MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Sandvik Kanthal AMPT Construction materials
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: Kanthal APMT is an advanced powder metallurgical, dispersion strengthened, ferritic Iron chromium aluminum alloy (FeCrAlMo alloy) recommended for continuous use up to 1250°C (2280°F) in oxidizing and reducing environments. Kanthal APMT has high creep strength and excellent form stability up to 1300°C. Kanthal APMT forms a protective and nonscaling Al O surface oxide when exposed to high temperature, which gives good protection in most furnace and combustion environments, i.e. oxidizing, sulphidizing and carburizing, as well as against attacks from deposits of coke, ash, etc. The combination of excellent oxidation properties and form stability makes the alloy unique. The superior resistance of Kanthal APMT to oxidation and carburization makes it very suitable for high temperature construction applications in various atmospheres.

Applications:

  • Radiation tubes for electrical and gas heated furnaces
  • Retorts and muffles for heat treatment and high-temperature sintering of powder metallurgical components
  • Shielding tubes
  • Burner components, nozzles and flame detectors
  • Load carriers, furnace furniture and load carrying trays
  • Radiant cracker tubes in ethylene furnaces
  • Uncooled components in coal, gas, and biofuel fired power plants
  • Thermocouple protection tubes in power plants and high temperature petrochemical processes

Information provided by Sandvik

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.25 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 250
Tensile Strength, Ultimate 725 - 780 MPa
 120 MPa
@Temperature 800 °C
 420 MPa
@Temperature 600 °C
Tensile Strength, Yield 510 - 600 MPa
@Strain 0.2 %
Elongation at Break 10 - 25 %
Creep Strength 0.900 MPa
@Temperature 1300 °C,
Time 3.60e+8 sec
1% Elongation
 1.10 MPa
@Temperature 1200 °C,
Time 3.60e+8 sec
1% Elongation
 1.20 MPa
@Temperature 1300 °C,
Time 3.60e+7 sec
1% Elongation
 1.50 MPa
@Temperature 1300 °C,
Time 3.60e+6 sec
1% Elongation
 1.60 MPa
@Temperature 1200 °C,
Time 3.60e+7 sec
1% Elongation
 2.10 MPa
@Temperature 1300 °C,
Time 360000 sec
1% Elongation
 2.30 MPa
@Temperature 1200 °C,
Time 3.60e+6 sec
1% Elongation
 2.60 MPa
@Temperature 1100 °C,
Time 3.60e+8 sec
1% Elongation
 3.40 MPa
@Temperature 1200 °C,
Time 360000 sec
1% Elongation
 3.60 MPa
@Temperature 1100 °C,
Time 3.60e+7 sec
1% Elongation
 5.00 MPa
@Temperature 1100 °C,
Time 3.60e+6 sec
1% Elongation
 6.10 MPa
@Temperature 1000 °C,
Time 3.60e+8 sec
1% Elongation
 7.00 MPa
@Temperature 1100 °C,
Time 360000 sec
1% Elongation
 7.80 MPa
@Temperature 1000 °C,
Time 3.60e+7 sec
1% Elongation
 9.90 MPa
@Temperature 1000 °C,
Time 3.60e+6 sec
1% Elongation
 10.8 MPa
@Temperature 900 °C,
Time 3.60e+8 sec
1% Elongation
 12.7 MPa
@Temperature 1000 °C,
Time 360000 sec
1% Elongation
 13.2 MPa
@Temperature 900 °C,
Time 3.60e+7 sec
1% Elongation
 16.2 MPa
@Temperature 900 °C,
Time 3.60e+6 sec
1% Elongation
 18.8 MPa
@Temperature 800 °C,
Time 3.60e+8 sec
1% Elongation
 19.7 MPa
@Temperature 900 °C,
Time 360000 sec
1% Elongation
 21.0 MPa
@Temperature 800 °C,
Time 3.60e+7 sec
1% Elongation
 23.4 MPa
@Temperature 800 °C,
Time 3.60e+6 sec
1% Elongation
 26.2 MPa
@Temperature 800 °C,
Time 360000 sec
1% Elongation
 31.4 MPa
@Temperature 700 °C,
Time 3.60e+8 sec
1% Elongation
 34.0 MPa
@Temperature 700 °C,
Time 3.60e+7 sec
1% Elongation
 36.8 MPa
@Temperature 700 °C,
Time 3.60e+6 sec
1% Elongation
 39.9 MPa
@Temperature 700 °C,
Time 360000 sec
1% Elongation
Rupture Strength 0.500 MPa
@Temperature 1300 °C,
Time 3.60e+8 sec
 0.800 MPa
@Temperature 1200 °C,
Time 3.60e+8 sec
 0.900 MPa
@Temperature 1300 °C,
Time 3.60e+7 sec
 1.40 MPa
@Temperature 1200 °C,
Time 3.60e+7 sec
 1.50 MPa
@Temperature 1300 °C,
Time 3.60e+6 sec
 2.30 MPa
@Temperature 1100 °C,
Time 3.60e+8 sec
 2.50 MPa
@Temperature 1200 °C,
Time 3.60e+6 sec
 2.70 MPa
@Temperature 1300 °C,
Time 360000 sec
 3.50 MPa
@Temperature 1100 °C,
Time 3.60e+7 sec
 4.60 MPa
@Temperature 1200 °C,
Time 360000 sec
 5.50 MPa
@Temperature 1100 °C,
Time 3.60e+6 sec
 6.10 MPa
@Temperature 1000 °C,
Time 3.60e+8 sec
 8.10 MPa
@Temperature 1000 °C,
Time 3.60e+7 sec
 8.70 MPa
@Temperature 1100 °C,
Time 360000 sec
 10.6 MPa
@Temperature 900 °C,
Time 3.60e+8 sec
 10.8 MPa
@Temperature 1000 °C,
Time 3.60e+6 sec
 13.4 MPa
@Temperature 900 °C,
Time 3.60e+7 sec
 14.4 MPa
@Temperature 1000 °C,
Time 360000 sec
 17.0 MPa
@Temperature 900 °C,
Time 3.60e+6 sec
 18.0 MPa
@Temperature 800 °C,
Time 3.60e+8 sec
 21.1 MPa
@Temperature 800 °C,
Time 3.60e+7 sec
 21.6 MPa
@Temperature 900 °C,
Time 360000 sec
 24.8 MPa
@Temperature 800 °C,
Time 3.60e+6 sec
 29.2 MPa
@Temperature 800 °C,
Time 360000 sec
 30.8 MPa
@Temperature 700 °C,
Time 3.60e+8 sec
 35.0 MPa
@Temperature 700 °C,
Time 3.60e+7 sec
 39.7 MPa
@Temperature 700 °C,
Time 3.60e+6 sec
 45.0 MPa
@Temperature 700 °C,
Time 360000 sec
Modulus of Elasticity 130 GPa
@Temperature 1000 °C
Young's
 150 GPa
@Temperature 800 °C
Young's
 170 GPa
@Temperature 600 °C
Young's
 190 GPa
@Temperature 400 °C
Young's
 205 GPa
@Temperature 200 °C
Young's
 210 GPa
@Temperature 100 °C
Young's
 220 GPa
@Temperature 20.0 °C
Young's
Poissons Ratio 0.30
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000140 ohm-cm
 0.0000100 ohm-cm
@Temperature 100 - 200 °C
 0.0000101 ohm-cm
@Temperature 300 - 500 °C
 0.0000103 ohm-cm
@Temperature 900 - 1200 °C
 0.0000104 ohm-cm
@Temperature 1300 °C
 0.0000105 ohm-cm
@Temperature 600 - 800 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.4 µm/m-°C
@Temperature 20.0 - 250 °C
 13.1 µm/m-°C
@Temperature 20.0 - 500 °C
 13.6 µm/m-°C
@Temperature 20.0 - 750 °C
 14.7 µm/m-°C
@Temperature 20.0 - 1000 °C
 15.4 µm/m-°C
@Temperature 20.0 - 1250 °C
Specific Heat Capacity 0.480 J/g-°C
@Temperature 20.0 °C
 0.560 J/g-°C
@Temperature 200 °C
 0.640 J/g-°C
@Temperature 400 °C
 0.670 J/g-°C
@Temperature 800 °C
 0.690 J/g-°C
@Temperature 1000 °C
 0.700 J/g-°C
@Temperature 1200 °C
 0.710 J/g-°C
@Temperature 600 °C
Thermal Conductivity 11.0 W/m-K
@Temperature 50.0 °C
 21.0 W/m-K
@Temperature 600 °C
 23.0 W/m-K
@Temperature 800 °C
 27.0 W/m-K
@Temperature 1000 °C
 29.0 W/m-K
@Temperature 1200 °C
Melting Point 1500 °C
Maximum Service Temperature, Air 1250 °C
Maximum Service Temperature, Inert 1250 °C
 
Optical PropertiesOriginal ValueComments
Emissivity (0-1) 0.70
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 5.0 %
Carbon, C <= 0.080 %
Chromium, Cr 20.5 - 23.5 %
Iron, Fe 67.32 - 71.5 %As Balance
Manganese, Mn <= 0.40 %
Molybdenum, Mo 3.0 %
Silicon, Si <= 0.70 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Special Metals INCONEL® Alloy 601
Sandvik Kanthal APM Resistance Strip
Sandvik Kanthal APM Construction materials
Carpenter MP35N* Ni-Co-Cr-Mo Alloy, 0% Cold Reduction

NSANDV5025 / 199589

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.