Physical Properties | Metric | English | Comments |
---|
Density | 8.25 g/cc | 0.298 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 311 @Temperature 760 °C | 311 @Temperature 1400 °F |
Hardness, Knoop | 335 @Temperature 760 °C | 335 @Temperature 1400 °F |
Hardness, Rockwell B | 88 @Temperature 760 °C | 88 @Temperature 1400 °F |
Hardness, Rockwell C | 33 @Temperature 760 °C | 33 @Temperature 1400 °F |
Hardness, Vickers | 323 @Temperature 760 °C | 323 @Temperature 1400 °F |
Tensile Strength, Ultimate | 865 MPa @Temperature 760 °C | 125000 psi @Temperature 1400 °F |
Tensile Strength, Yield | 687 MPa @Strain 0.2 %, Temperature 760 °C | 99600 psi @Strain 0.2 %, Temperature 1400 °F |
Elongation at Break | 8.0 % @Temperature 760 °C | 8.0 % @Temperature 1400 °F |
Modulus of Elasticity | 150 GPa @Temperature 927 °C | 21800 ksi @Temperature 1700 °F |
| 160 GPa @Temperature 871 °C | 23200 ksi @Temperature 1600 °F |
| 163 GPa @Temperature 843 °C | 23600 ksi @Temperature 1550 °F |
| 166 GPa @Temperature 816 °C | 24100 ksi @Temperature 1500 °F |
| 171 GPa @Temperature 760 °C | 24800 ksi @Temperature 1400 °F |
| 178 GPa @Temperature 677 °C | 25800 ksi @Temperature 1250 °F |
| 179 GPa @Temperature 649 °C | 26000 ksi @Temperature 1200 °F |
| 182 GPa @Temperature 593 °C | 26400 ksi @Temperature 1100 °F |
| 188 GPa @Temperature 538 °C | 27300 ksi @Temperature 1000 °F |
| 190 GPa @Temperature 482 °C | 27600 ksi @Temperature 900 °F |
| 198 GPa @Temperature 371 °C | 28700 ksi @Temperature 700 °F |
| 204 GPa @Temperature 260 °C | 29600 ksi @Temperature 500 °F |
| 213 GPa @Temperature 149 °C | 30900 ksi @Temperature 300 °F |
| 218 GPa @Temperature 27.0 °C | 31600 ksi @Temperature 80.6 °F |
Poissons Ratio | 0.31 @Temperature 149 °C | 0.31 @Temperature 300 °F |
| 0.31 @Temperature 27.0 °C | 0.31 @Temperature 80.6 °F |
| 0.32 @Temperature 482 °C | 0.32 @Temperature 900 °F |
| 0.32 @Temperature 371 °C | 0.32 @Temperature 700 °F |
| 0.32 @Temperature 260 °C | 0.32 @Temperature 500 °F |
| 0.33 @Temperature 760 °C | 0.33 @Temperature 1400 °F |
| 0.33 @Temperature 677 °C | 0.33 @Temperature 1250 °F |
| 0.33 @Temperature 649 °C | 0.33 @Temperature 1200 °F |
| 0.34 @Temperature 843 °C | 0.34 @Temperature 1550 °F |
| 0.35 @Temperature 927 °C | 0.35 @Temperature 1700 °F |
Shear Modulus | 55.0 GPa @Temperature 927 °C | 7980 ksi @Temperature 1700 °F |
| 61.0 GPa @Temperature 843 °C | 8850 ksi @Temperature 1550 °F |
| 64.0 GPa @Temperature 760 °C | 9280 ksi @Temperature 1400 °F |
| 67.0 GPa @Temperature 677 °C | 9720 ksi @Temperature 1250 °F |
| 69.0 GPa @Temperature 593 °C | 10000 ksi @Temperature 1100 °F |
| 72.0 GPa @Temperature 482 °C | 10400 ksi @Temperature 900 °F |
| 75.0 GPa @Temperature 371 °C | 10900 ksi @Temperature 700 °F |
| 77.0 GPa @Temperature 260 °C | 11200 ksi @Temperature 500 °F |
| 81.0 GPa @Temperature 149 °C | 11700 ksi @Temperature 300 °F |
| 83.0 GPa @Temperature 27.0 °C | 12000 ksi @Temperature 80.6 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Magnetic Permeability | <= 1.002 @Temperature 21.0 °C | <= 1.002 @Temperature 69.8 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 13.5 µm/m-°C @Temperature 21.0 - 538 °C | 7.50 µin/in-°F @Temperature 69.8 - 1000 °F |
| 14.0 µm/m-°C @Temperature 21.0 - 649 °C | 7.78 µin/in-°F @Temperature 69.8 - 1200 °F |
| 14.8 µm/m-°C @Temperature 21.0 - 760 °C | 8.22 µin/in-°F @Temperature 69.8 - 1400 °F |
| 15.2 µm/m-°C @Temperature 21.0 - 871 °C | 8.44 µin/in-°F @Temperature 69.8 - 1600 °F |
| 16.3 µm/m-°C @Temperature 21.0 - 927 °C | 9.06 µin/in-°F @Temperature 69.8 - 1700 °F |
| 16.8 µm/m-°C @Temperature 21.0 - 982 °C | 9.33 µin/in-°F @Temperature 69.8 - 1800 °F |
Specific Heat Capacity | 0.452 J/g-°C @Temperature 21.0 °C | 0.108 BTU/lb-°F @Temperature 69.8 °F |
Thermal Conductivity | 11.5 W/m-K @Temperature 149 °C | 79.8 BTU-in/hr-ft²-°F @Temperature 300 °F |
| 12.5 W/m-K @Temperature 204 °C | 86.8 BTU-in/hr-ft²-°F @Temperature 399 °F |
| 13.6 W/m-K @Temperature 260 °C | 94.4 BTU-in/hr-ft²-°F @Temperature 500 °F |
| 14.7 W/m-K @Temperature 316 °C | 102 BTU-in/hr-ft²-°F @Temperature 601 °F |
| 16.8 W/m-K @Temperature 427 °C | 117 BTU-in/hr-ft²-°F @Temperature 801 °F |
| 18.8 W/m-K @Temperature 538 °C | 130 BTU-in/hr-ft²-°F @Temperature 1000 °F |
| 20.0 W/m-K @Temperature 593 °C | 139 BTU-in/hr-ft²-°F @Temperature 1100 °F |
| 21.0 W/m-K @Temperature 644 °C | 146 BTU-in/hr-ft²-°F @Temperature 1190 °F |
| 22.0 W/m-K @Temperature 704 °C | 153 BTU-in/hr-ft²-°F @Temperature 1300 °F |
| 23.1 W/m-K @Temperature 760 °C | 160 BTU-in/hr-ft²-°F @Temperature 1400 °F |
| 24.1 W/m-K @Temperature 816 °C | 167 BTU-in/hr-ft²-°F @Temperature 1500 °F |
| 25.1 W/m-K @Temperature 871 °C | 174 BTU-in/hr-ft²-°F @Temperature 1600 °F |
Melting Point | 1310 - 1345 °C | 2390 - 2453 °F |
Solidus | 1310 °C | 2390 °F |
Liquidus | 1335 °C | 2435 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Aluminum, Al | 1.4 - 1.6 % | 1.4 - 1.6 % |
Boron, B | 0.0030 - 0.010 % | 0.0030 - 0.010 % |
Carbon, C | 0.050 - 0.12 % | 0.050 - 0.12 % |
Chromium, Cr | 18 - 20 % | 18 - 20 % |
Cobalt, Co | 10 - 12 % | 10 - 12 % |
Iron, Fe | <= 5.0 % | <= 5.0 % |
Manganese, Mn | <= 0.10 % | <= 0.10 % |
Molybdenum, Mo | 9.0 - 10.5 % | 9.0 - 10.5 % |
Nickel, Ni | 53 % | 53 % |
Silicon, Si | <= 0.50 % | <= 0.50 % |
Sulfur, S | <= 0.015 % | <= 0.015 % |
Titanium, Ti | 3.0 - 3.3 % | 3.0 - 3.3 % |