MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Versalis Riblene® FF 34 F Film Grade Low Density Polyethylene
Categories: Polymer; Thermoplastic; Polyethylene (PE); Low Density (LDPE); Low Density Polyethylene (LDPE), Film Grade

Material Notes: Riblene FF 34 F is a high molecular weight LDPE, with slip and antiblocking agent, suitable for blown film extrusion. Riblene FF 34 F is characterized by a good melt strength leading to a good bubble stability during extrusion. Films manufactured by Riblene FF 34 F are easily heat shrinkable and characterized by good mechanical properties. Applications: Riblene FF 34 F is recommended for the production of general packaging film, shoppers, lamination film and blend.

Property values reported for film extruded with BUR 1:3, thickness 70 µm. Actual properties are typical and may vary depending upon operating conditions and additive package.

Information provided by Versalis.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.923 g/cc0.0333 lb/in³ISO 1183
Thickness 70.0 microns2.76 milAs-tested; BUR 1:3
 30.0 - 120 microns1.18 - 4.72 milRecommended
Melt Flow 0.80 g/10 min
@Load 2.16 kg,
Temperature 190 °C
0.80 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 10.0 MPa1450 psiISO 527-3
Film Tensile Strength at Yield, TD 11.0 MPa1600 psiISO 527-3
Film Elongation at Break, MD 400 %400 %ISO 527-3
Film Elongation at Break, TD 600 %600 %ISO 527-3
Coefficient of Friction, Dynamic >= 0.11>= 0.11ISO 8295
Elmendorf Tear Strength, MD 4.60 g/micron117 g/milISO 6383-2
Elmendorf Tear Strength, TD 6.10 g/micron155 g/milISO 6383-2
Dart Drop Test 180 g0.397 lbF50; ISO 7765-1/A
Film Tensile Strength at Break, MD 22.0 MPa3190 psiISO 527-3
Film Tensile Strength at Break, TD 19.0 MPa2760 psiISO 527-3
1% Secant Modulus, MD 180 MPa26100 psiISO 527-3
1% Secant Modulus, TD 190 MPa27600 psiISO 527-3
 
Thermal PropertiesMetricEnglishComments
Melting Point 114 °C237 °FManufacturer method
Vicat Softening Point 95.0 °C
@Load 1.00 kg
203 °F
@Load 2.20 lb
ISO 306/A
Brittleness Temperature <= -75.0 °C<= -103 °FASTM D 746
 
Optical PropertiesMetricEnglishComments
Haze 9.0 %9.0 %ISO 14782
Gloss 60 %60 %45°; ASTM D 2457
 
Processing PropertiesMetricEnglishComments
Processing Temperature 170 - 200 °C338 - 392 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PENF9806 / 265684

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.