MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Polymer Resources PPX-EN-FR3 Modified-PPO, V-1 Flame Retardant, Extrusion Grade
Categories: Polymer; Thermoplastic; Polyphenylene Ether/PPO; Polyphenylene Ether, Heat Resistant

Material Notes: Modified-Polyphenylene Oxide, V-1 Flame Retardant, 265F HDT, Extrusion Grade

Features: • Bromine Free • Chlorine Free
Process: Extrusion
Notes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples.

Information provided by Polymer Resources Corporation.

Key Words: UL E113219; Polyphenylene Ether + PS
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.06 g/ccASTM D792
Linear Mold Shrinkage 0.0050 - 0.0070 cm/cmASTM D955
Melt Flow 4.0 - 8.0 g/10 min
@Load 11.6 kg,
Temperature 250 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 119ASTM D785
Tensile Strength at Break 9000 psiASTM D638
Tensile Strength, Yield 9300 psiASTM D638
Flexural Strength 13000 psiASTM D790
Flexural Modulus 350 ksiASTM D790
Izod Impact, Notched 2.50 ft-lb/in
@Temperature -40.0 °C
ASTM D256
 4.00 ft-lb/in
@Temperature 22.8 °C
ASTM D256
Gardner Impact 150 in-lbASTM D3029
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+17 ohm-cmASTM D257
Dielectric Strength 610 V/mil
@Thickness 3.00 mm
ASTM D149
Comparative Tracking Index 250 - 400 VUL 746
Hot Wire Ignition, HWI >= 120 sec
@Thickness 1.50 mm
UL 746
 >= 120 sec
@Thickness 1.70 mm
UL 746
 >= 120 sec
@Thickness 3.00 mm
UL 746
High Amp Arc Ignition, HAI 60 - 120 arcs
@Thickness 1.50 mm
UL 746
 60 - 120 arcs
@Thickness 1.70 mm
UL 746
 60 - 120 arcs
@Thickness 3.00 mm
UL 746
High Voltage Arc-Tracking Rate, HVTR 80.0 - 150 mm/minUL 746
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 265 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 250 °FASTM D648
UL RTI, Electrical 149 °F
@Thickness 0.749 mm
UL 746
 230 °F
@Thickness 1.50 mm
UL 746
 230 °F
@Thickness 1.70 mm
UL 746
 230 °F
@Thickness 3.00 mm
UL 746
UL RTI, Mechanical with Impact 149 °F
@Thickness 0.749 mm
UL 746
 230 °F
@Thickness 1.50 mm
UL 746
 230 °F
@Thickness 1.70 mm
UL 746
 230 °F
@Thickness 3.00 mm
UL 746
UL RTI, Mechanical without Impact 149 °F
@Thickness 0.749 mm
UL 746
 221 °F
@Thickness 1.50 mm
UL 746
 221 °F
@Thickness 1.70 mm
UL 746
 221 °F
@Thickness 3.00 mm
UL 746
Flammability, UL94 V-1
@Thickness 1.50 mm
 V-1
@Thickness 3.00 mm
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature >= 400 °F
Middle Barrel Temperature >= 440 °F
Front Barrel Temperature >= 440 °F
Melt Temperature 440 - 490 °F
Drying Temperature 220 - 230 °F
Dry Time 3.00 - 4.00 hour
Vent Depth 0.00100 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Mitsubishi Iupital® A10-03 Copolymer Acetal
Ineos N01N-00 Polypropylene Impact Copolymer
Ineos N01G-02 Polypropylene Impact Copolymer
Ineos N00N-00 Polypropylene Impact Copolymer
Ineos N00M-00 Polypropylene Impact Copolymer

PPOLYQ206 / 160727

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.