MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Sandvik 19.12.3.Nb Welding wire
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: Sandvik 19.12.3.NbSi is a filler material suitable for joining chromium nickel molybdenum steels, stabilized or non stabilized, e.g. ASTM 316Ti, 316 and 316L for service temperatures up to 400 C (750 F). Sandvik 19.12.3.NbSi is used for MIG/MAG, TIG and Plasma arc welding.

Information provided by Sandvik

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.00 g/cc0.289 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers 220220
Tensile Strength, Ultimate  540 MPa
@Temperature 400 °C
78300 psi
@Temperature 752 °F
 610 MPa
@Temperature 20.0 °C
88500 psi
@Temperature 68.0 °F
Tensile Strength, Yield  390 MPa
@Strain 0.2 %,
Temperature 400 °C
56600 psi
@Strain 0.2 %,
Temperature 752 °F
 400 MPa
@Strain 0.2 %,
Temperature 20.0 °C
58000 psi
@Strain 0.2 %,
Temperature 68.0 °F
Elongation at Break  30 %
@Temperature 400 °C
30 %
@Temperature 752 °F
 36 %
@Temperature 20.0 °C
36 %
@Temperature 68.0 °F
Reduction of Area 59 %59 %
Creep Strength  45.0 MPa
@Temperature 20.0 °C
6530 psi
@Temperature 68.0 °F
 155 MPa
@Temperature 700 °C
22500 psi
@Temperature 1290 °F
Charpy Impact  60.0 J
@Temperature -196 °C
44.3 ft-lb
@Temperature -321 °F
 135 J
@Temperature 20.0 °C
99.6 ft-lb
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear 18.0 µm/m-°C
@Temperature 20.0 - 400 °C
10.0 µin/in-°F
@Temperature 68.0 - 752 °F
Thermal Conductivity  15.0 W/m-K
@Temperature 20.0 °C
104 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 15.0 W/m-K
@Temperature 100 °C
104 BTU-in/hr-ft²-°F
@Temperature 212 °F
 21.0 W/m-K
@Temperature 300 °C
146 BTU-in/hr-ft²-°F
@Temperature 572 °F
 23.0 W/m-K
@Temperature 500 °C
160 BTU-in/hr-ft²-°F
@Temperature 932 °F
Maximum Service Temperature, Air 400 °C752 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.030 %0.030 %All Weld Metal
 0.040 %0.040 %Nominal
 0.040 %0.040 %AIM
Chromium, Cr 18 %18 %All Weld Metal
 18.5 %18.5 %Nominal
 18.5 %18.5 %AIM
Cobalt, Co <= 0.20 %<= 0.20 %Nominal
 <= 0.20 %<= 0.20 %AIM
Copper, Cu <= 0.20 %<= 0.20 %Nominal
 <= 0.20 %<= 0.20 %AIM
Manganese, Mn 1.3 %1.3 %All Weld Metal
 1.5 %1.5 %Nominal
 1.5 %1.5 %AIM
Molybdenum, Mo 2.6 %2.6 %All Weld Metal
 2.6 %2.6 %Nominal
 2.6 %2.6 %AIM
Nickel, Ni 11 %11 %All Weld Metal
 11.5 %11.5 %Nominal
 11.5 %11.5 %AIM
Niobium, Nb (Columbium, Cb) 0.55 %0.55 %All Weld Metal
 >= 12 %>= 12 %Nominal
 >= 12 %>= 12 %AIM
Nitrogen, N 0.050 %0.050 %All Weld Metal
 <= 0.060 %<= 0.060 %Nominal
 <= 0.060 %<= 0.060 %AIM
Phosphorus, P 0.012 %0.012 %All Weld Metal
 <= 0.025 %<= 0.025 %Nominal
 <= 0.025 %<= 0.025 %AIM
Silicon, Si 0.40 %0.40 %All Weld Metal
 0.40 %0.40 %Nominal
 0.40 %0.40 %AIM
Sulfur, S 0.011 %0.011 %All Weld Metal
 <= 0.015 %<= 0.015 %Nominal
 <= 0.015 %<= 0.015 %AIM

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Universal Wire Works ER90SB-9 Steel Welding Wire
SSAB Tunnplat Domex® 315MC HSLA Steel
Bethlehem Steel BETHSTAR Grade 50 1/4 to 2-1/2 in. thick, killed steel plate
ASTM A736 Low Alloy Steel, Grade C, Class 1
ASTM A735 Low Alloy Steel, Class 1

NSANDV5088 / 199652

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.