MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Chosun Refractories SC40 Bricks, Oxide Bonded SiC
Categories: Ceramic; Carbide

Material Notes:

Information provided by Chosun Refractories via Korea Institute of Ceramic Engineering and Technology (KICET).

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 2.55 g/cc
Porosity 17 %
 
Mechanical PropertiesOriginal ValueComments
Modulus of Rupture 0.00981 GPa
@Temperature 1400 °C
 0.014715 GPa
@Temperature 250 °C
Compressive Strength 700 kg(f)/cm²Cold Crushing Strength
 
Thermal PropertiesOriginal ValueComments
CTE, linear 5.40 µm/m-°C
@Temperature 1000 °C
 
Component Elements PropertiesOriginal ValueComments
Fe2O3 1.6 %
SiC 42 %
 
Descriptive Properties
Refractories Under Load(2kg/cm²,T2°C)1,450

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chosun Refractories AB10L Alumina Magnesia Carbon Bricks for Ladle Wall And Bottom
Sharadaa Ceramics 26 Insulation Bricks-ASTM
Skamol Group SUPER 1100 ET Calcium Silicate Insulating Slab
Chosun Refractories L8S Magnesia Carbon Bricks for Ladle Slag Line
Chosun Refractories AM10L Alumina Magnesia Carbon Bricks for Ladle Wall And Bottom

CCHOS058 / 124002

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.