MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
SABIC LEXAN™ FR FL905 PC (Europe)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LEXAN FL905 Polycarbonate (PC) is an injection moldable non-chlorinated/brominated, 5% glass filled, foamable flame retardant grade with good impact performance. It has an MVR of 3(300°C/1.2kg), UL94 V0@3mm, and 5VA @6.0mm.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.20 g/ccASTM D792
Density 1.20 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.0060 cm/cm
@Thickness 3.20 mm
SABIC method
Linear Mold Shrinkage, Transverse 0.0050 cm/cm
@Thickness 3.20 mm
SABIC method
Melt Flow 3.0 g/10 min
@Load 1.20 kg,
Temperature 300 °C
cm³/10 min; ISO 1133
 3.2 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 44.0 MPa50 mm/min; ISO 527
 47.0 MPa50 mm/min; ASTM D638
Tensile Strength, Yield 57.0 MPa50 mm/min; ISO 527
 58.0 MPa50 mm/min; ASTM D638
Elongation at Break 25 %50 mm/min; ISO 527
 30 %50 mm/min; ASTM D638
Elongation at Yield 5.7 %50 mm/min; ASTM D638
 5.9 %50 mm/min; ISO 527
Tensile Modulus 2790 MPa1mm/min; ISO 527
 2810 MPa50 mm/min; ASTM D638
Flexural Yield Strength 91.0 MPa2 mm/min; ISO 178
 98.0 MPa1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2670 MPa1.3 mm/min, 50 mm span; ASTM D790
 2680 MPa2 mm/min; ISO 178
Izod Impact, Notched 520 J/mASTM D256
 137 J/m
@Temperature -30.0 °C
ASTM D256
Izod Impact, Notched (ISO) 27.0 kJ/m²80*10*3; ISO 180/1A
 12.0 kJ/m²
@Temperature -30.0 °C
80*10*3; ISO 180/1A
Izod Impact, Unnotched (ISO) 171 kJ/m²80*10*3; ISO 180/1U
 172 kJ/m²
@Temperature -30.0 °C
80*10*3; ISO 180/1U
Charpy Impact Unnotched 335 kJ/m²Edgew 80*10*3 sp=62mm; ISO 179/1eU
 313 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*3 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 31.0 kJ/m²Edgew 80*10*3 sp=62mm; ISO 179/1eA
 16.0 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*3 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 53.0 JASTM D3763
 46.0 J
@Temperature -30.0 °C
ASTM D3763
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 52.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
 54.0 µm/m-°C
@Temperature -40.0 - 95.0 °C
ASTM E831
CTE, linear, Transverse to Flow 76.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
 80.0 µm/m-°C
@Temperature -40.0 - 95.0 °C
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 145 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 146 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 134 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 140 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 147 °CRate B/50; ISO 306
 148 °CRate A/50; ASTM D1525
 149 °CRate B/120; ISO 306
Flammability, UL94 V-0
@Thickness 3.00 mm
UL 94
 5VA
@Thickness 6.00 mm
UL 94
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 290 - 310 °CInjection Molding
Zone 1 270 - 295 °C
Zone 2 280 - 305 °C
Zone 3 295 - 315 °C
Melt Temperature 295 - 315 °C
Mold Temperature 70.0 - 95.0 °C
Drying Temperature 120 °CInjection Molding
Dry Time 3.00 - 4.00 hourInjection Molding
 48.0 hourCumulative; Injection Molding
Moisture Content 0.020 %
Back Pressure 0.300 - 0.700 MPa
Shot Size 40 - 60 %
Vent Depth 0.00200 - 0.00760 cm
Screw Speed 40 - 70 rpm
 
Descriptive Properties
FOAM - Flame Class Minimum Density0.9 g/cm³

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABI10638 / 244105

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.