MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Aluminum 6061-T6; 6061-T651  (Unverified Data**)
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 6000 Series Aluminum Alloy

Material Notes: General 6061 characteristics and uses: Excellent joining characteristics, good acceptance of applied coatings. Combines relatively high strength, good workability, and high resistance to corrosion; widely available. The T8 and T9 tempers offer better chipping characteristics over the T6 temper.

Applications: Aircraft fittings, camera lens mounts, couplings, marines fittings and hardware, electrical fittings and connectors, decorative or misc. hardware, hinge pins, magneto parts, brake pistons, hydraulic pistons, appliance fittings, valves and valve parts; bike frames.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: al6061, UNS A96061; ISO AlMg1SiCu; Aluminium 6061-T6, AD-33 (Russia); AA6061-T6; 6061T6, ISO AlMg1SiCu; Aluminium 6061-T651, AD-33 (Russia); AA6061-T651; Al6061-T6
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.70 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 95AA; Typical; 500 g load; 10 mm ball
Hardness, Knoop 120Converted from Brinell Hardness Value
Hardness, Rockwell A 40Converted from Brinell Hardness Value
Hardness, Rockwell B 60Converted from Brinell Hardness Value
Hardness, Vickers 107Converted from Brinell Hardness Value
Tensile Strength, Ultimate 45.0 ksiAA; Typical
 24.0 MPa
@Temperature 371 °C
 32.0 MPa
@Temperature 316 °C
 51.0 MPa
@Temperature 260 °C
 131 MPa
@Temperature 204 °C
 234 MPa
@Temperature 149 °C
 290 MPa
@Temperature 100 °C
 310 MPa
@Temperature 24.0 °C
 324 MPa
@Temperature -28.0 °C
 338 MPa
@Temperature -80.0 °C
 414 MPa
@Temperature -196 °C
Tensile Strength, Yield 40.0 ksiAA; Typical
 12.0 MPa
@Strain 0.2 %,
Temperature 371 °C
 19.0 MPa
@Strain 0.2 %,
Temperature 316 °C
 34.0 MPa
@Strain 0.2 %,
Temperature 260 °C
 103 MPa
@Strain 0.2 %,
Temperature 204 °C
 214 MPa
@Strain 0.2 %,
Temperature 149 °C
 262 MPa
@Strain 0.2 %,
Temperature 100 °C
 276 MPa
@Strain 0.2 %,
Temperature 24.0 °C
 283 MPa
@Strain 0.2 %,
Temperature -28.0 °C
 290 MPa
@Strain 0.2 %,
Temperature -80.0 °C
 324 MPa
@Strain 0.2 %,
Temperature -196 °C
Elongation at Break 17 %
@Temperature -28.0 °C
 17 %
@Temperature 24.0 °C
 18 %
@Temperature -80.0 °C
 18 %
@Temperature 100 °C
 20 %
@Temperature 149 °C
 22 %
@Temperature -196 °C
 28 %
@Temperature 204 °C
 60 %
@Temperature 260 °C
 85 %
@Temperature 316 °C
 95 %
@Temperature 371 °C
 12 %
@Thickness 1.59 mm
AA; Typical
 17 %
@Diameter 12.7 mm
AA; Typical
Modulus of Elasticity 10000 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Notched Tensile Strength 324 MPa2.5 cm width x 0.16 cm thick side-notched specimen, Kt = 17.
Ultimate Bearing Strength 607 MPaEdge distance/pin diameter = 2.0
Bearing Yield Strength 386 MPaEdge distance/pin diameter = 2.0
Poissons Ratio 0.33Estimated from trends in similar Al alloys.
Fatigue Strength 14000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Fracture Toughness 29.0 MPa-m½KIC; TL orientation.
Machinability 50 %0-100 Scale of Aluminum Alloys
Shear Modulus 26.0 GPaEstimated from similar Al alloys.
Shear Strength 30.0 ksiAA; Typical
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 24.0 ohm-cir-mil/ft
@Temperature 20.0 °C
AA; Typical
 
Thermal PropertiesOriginal ValueComments
CTE, linear 13.1 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 25.2 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.896 J/g-°C
Thermal Conductivity 1160 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 1080 - 1205 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting can be eliminated by homogenization.
Solidus 1080 °FAA; Typical
Liquidus 1205 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Solution Temperature 985 °F
Aging Temperature 320 °FRolled or drawn products; hold at temperature for 18 hr
 350 °FExtrusions or forgings; hold at temperature for 8 hr
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 95.8 - 98.6 %As remainder
Chromium, Cr 0.04 - 0.35 %
Copper, Cu 0.15 - 0.40 %
Iron, Fe <= 0.70 %
Magnesium, Mg 0.80 - 1.2 %
Manganese, Mn <= 0.15 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si 0.40 - 0.80 %
Titanium, Ti <= 0.15 %
Zinc, Zn <= 0.25 %

References for this datasheet.

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 6061-T6; 6061-T651
Aluminum 7075-T6; 7075-T651
Aluminum 6063-T6
Aluminum 6351-T6; 6351-T651
Aluminum 6061-O

MA6061T6 / 9391

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.