MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Daikin DAI-EL® G-603 Fluoroelastomer Terpolymer, Bisphenol Curable Grade, 71% Fluorine Content
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: DAI-EL® G-603 is a medium Mooney viscosity, bisphenol cure incorporated terpolymer designed for transfer and compression molding applications. DAI-EL® G-603 provides excellent chemical and solvent resistance and very low fuel permeation rates.

Typical Applications: O-rings, gaskets and seals in fuel systems

Rheological Properties MDR 2000:
Temperature: 190°C
Frequency: 100 cpm
Strain: 0.5°
Test time: 6 min

Information provided by Daikin.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.90 g/cc1.90 g/cc
Mooney Viscosity 31
@Temperature 121 °C
31
@Temperature 250 °F
ML 1+10
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7979
Tensile Strength at Break 12.3 MPa1780 psi
Elongation at Break 220 %220 %
100% Modulus 5.60 MPa
@Strain 100 %
812 psi
@Strain 100 %
Compression Set  41 %
@Temperature 175 °C,
Time 252000 sec
41 %
@Temperature 347 °F,
Time 70.0 hour
#214 O-ring; ASTM D395 Method B
 50 %
@Temperature 200 °C,
Time 252000 sec
50 %
@Temperature 392 °F,
Time 70.0 hour
#214 O-ring; ASTM D395 Method B
 
Thermal PropertiesMetricEnglishComments
Minimum Service Temperature, Air -8.00 °C17.6 °FLow Temperature Retraction, TR10
 -4.80 °C23.4 °FGehman Torsion T10; ASTM 1053-92A
 -2.00 °C28.4 °FLow Temperature Retraction, TR70
 -1.30 °C29.7 °FGehman Torsion T2; ASTM 1053-92A
Brittleness Temperature -14.0 °C6.80 °FEmbrittlement
 
Processing PropertiesMetricEnglishComments
Cure Time 0.700 min0.0117 hourts2, scorch time
 1.10 min0.0183 hourt'50, time to 50% cure
 2.40 min0.0400 hourt'90, time to 90% cure
 10.0 min
@Temperature 190 °C
0.167 hour
@Temperature 374 °F
Press Cure
 1440 min
@Temperature 232 °C
24.0 hour
@Temperature 450 °F
Post cure
 
Component Elements PropertiesMetricEnglishComments
Fluorine, F 71 %71 %
 
Descriptive Properties
ColorWhite to light pink sheet
MH11.3 dNmmaximum torque
ML0.7 dNmminimum torque
Test Formula100 phrDAI-EL® G-603
 3 phrMagnesium oxide
 30 phrMT Carbon Black (N-990)
 6 phrCalcium hydroxide

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PDAIJ9848 / 209919

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.