MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Mid-Mountain Materials CERMEX® BK2200SW Low Biopersistence Thermal Insulation Blanket
Categories: Ceramic; Glass; Glass Fiber; Oxide; Silicon Oxide; Other Engineering Material; Composite Fibers

Material Notes: Alkaline Earth Silicate Wool, Needled Blanket

Information provided by Mid-Mountain Materials

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 6.00 lb/ft³
 8.00 lb/ft³
Thickness 6250 - 50000 microns
 
Thermal PropertiesOriginal ValueComments
Thermal Conductivity 0.0600 W/m-K
@Temperature 260 °C
 0.130 W/m-K
@Temperature 538 °C
 0.220 W/m-K
@Temperature 816 °C
 0.280 W/m-K
@Temperature 982 °C
Melting Point 1499 °C
Maximum Service Temperature, Air 2200 °FContinuous
Shrinkage <= 2.0 %
@Temperature 651.1 °C,
Time 86400 sec
 
Component Elements PropertiesOriginal ValueComments
CaO 16 - 22 %
MgO 12 - 19 %
SiO2 60 - 70 %
 
Descriptive Properties
Al2O3 (%)Trace
ColorWhite
Width (in)24
 48

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Mid-Mountain Materials CERMEX® BK1800SW Low Biopersistence Thermal Insulation Blanket
E-Glass Fiber, Generic
S-2 Glass® Fiber
S-Glass Fiber, Generic
DuPont™ Kevlar® 49 Aramid Fiber

CMID62 / 141230

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.