MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Aronkasei AR-BOEX-60 Alloy
Categories: Polymer; Thermoplastic

Material Notes: Characteristics:
  • Over molding with a polar resin such as ABS, PC, and others.
  • Excellent extrusion molding properties
Examples of Use: Building materials door stops, baseboard members, and others.

Information provided by ARONKASEI CO.,LTD Elastomer Dept.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.05 g/cc1.05 g/ccJIS K 7112
Linear Mold Shrinkage 0.0010 - 0.060 cm/cm0.0010 - 0.060 in/in
Melt Flow 0.10 g/10 min
@Load 2.16 kg,
Temperature 190 °C
0.10 g/10 min
@Load 4.77 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6363JIS K 6253 A
Tensile Strength at Break 8.80 MPa1280 psiJIS K 6251
Elongation at Break 560 %560 %JIS K 6251
300% Modulus 3.90 MPa566 psiJIS K 6251
Resilience 6565[%]; JIS K 6255
Tear Strength 37.0 kN/m211 pliJIS K 6252
Taber Abrasion, mg/1000 Cycles 390
@Load 0.999 kg
390
@Load 2.20 lb
[mg], H-22; JIS K 6264
Compression Set  23 %
@Temperature 23.0 °C,
Time 86400 sec
23 %
@Temperature 73.4 °F,
Time 24.0 hour
JIS K 6262
 64 %
@Temperature 70.0 °C,
Time 86400 sec
64 %
@Temperature 158 °F,
Time 24.0 hour
JIS K 6262
 86 %
@Temperature 100 °C,
Time 86400 sec
86 %
@Temperature 212 °F,
Time 24.0 hour
JIS K 6262
 
Thermal PropertiesMetricEnglishComments
Softening Point 82.0 °C180 °F
Brittleness Temperature <= -60.0 °C<= -76.0 °FJIS K 6261
 
Descriptive Properties
ColorMilky-White (Natural)
Molding MethodExtrusion

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PJARON030 / 293942

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.