MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Morgan Advanced Ceramics Kaowool 2600 Organic RCF Vacuum Formed Thermal Ceramic
Categories: Ceramic; Oxide

Material Notes: Vacuum formed products are rigid, self-supporting fiber insulation manufactured from a slurry of ceramic fibers, binders and other proprietary ingredients. Customers are provided with optimized, engineered solutions from our wide range of formulations. Kaowool 2600 uses high temperature alumina fibers in the manufacturing process. It is an excellent dimensionally stable product and has minimal shrinkage at its use limit of 2700°F (1510°C).

Information provided by Morgan Advanced Materials

Key Words: Thermal Ceramics
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.0150 g/cc
 
Mechanical PropertiesOriginal ValueComments
Modulus of Rupture 0.00790 GPa
Compressive Strength 0.210 MPaat 5% deformation
 0.280 MPaat 10% deformation
 
Thermal PropertiesOriginal ValueComments
Thermal Conductivity 0.0800 W/m-K
@Temperature 260 °C
ASTM C201
 0.100 W/m-K
@Temperature 538 °C
ASTM C201
 0.150 W/m-K
@Temperature 816 °C
ASTM C201
 0.220 W/m-K
@Temperature 1093 °C
ASTM C201
Maximum Service Temperature, Air 1426 °CContinuous Use
 1482 °C
Shrinkage 0.30 %
@Temperature 816 °C,
Time 86400 sec
 0.30 %
@Temperature 982 °C,
Time 86400 sec
 0.60 %
@Temperature 1093 °C,
Time 86400 sec
 0.70 %
@Temperature 1204 °C,
Time 86400 sec
 0.80 %
@Temperature 1316 °C,
Time 86400 sec
 
Component Elements PropertiesOriginal ValueComments
Al2O3 51 %
Loss on Ignition(%) 7.0 - 9.0 %
Other <= 1.0 %
 6.0 - 8.0 %organic
SiO2 49 %
 
Descriptive Properties
Colorblue

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Morgan Advanced Ceramics Kaowool A Organic RCF Vacuum Formed Thermal Ceramic
Morgan Advanced Ceramics Kaowool 80 Organic RCF Vacuum Formed Thermal Ceramic
Morgan Advanced Ceramics Kaowool 3000 Organic RCF Vacuum Formed Thermal Ceramic
Morgan Advanced Ceramics Green Glass Paper Thermal Ceramic
Morgan Advanced Ceramics Ceramic Fiber Papers STD Paper Ceramic Fiber

CMORF70121 / 203419

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.