MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Teijin Panlite® LV-2250Z Transparent and Weather Resistant grade Polycarbonate Resin
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Molded

Material Notes: Typical injection molding grade that has weather resistance and is bluish-tinted to exhibit clear color.

Applications:

  • Components of electric, electronic, business machine and industrial equipment components that need flame retardancy, transparency and weather resistance
  • Information provided by Teijin Chemicals Ltd.

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Density 1.20 g/cc0.0434 lb/in³ISO 1183
    Moisture Absorption 0.200 %
    @Temperature 23.0 °C,
    Time 86400 sec
    0.200 %
    @Temperature 73.4 °F,
    Time 24.0 hour
    ISO 62
    Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
    @Thickness 4.00 mm
    0.0050 - 0.0070 in/in
    @Thickness 0.157 in
    Teijin method
    Linear Mold Shrinkage, Transverse 0.0050 - 0.0070 cm/cm
    @Thickness 4.00 mm
    0.0050 - 0.0070 in/in
    @Thickness 0.157 in
    Teijin method
    Melt Flow 9.6 g/10 min
    @Load 1.20 kg,
    Temperature 300 °C
    9.6 g/10 min
    @Load 2.65 lb,
    Temperature 572 °F
    ISO 1133
     
    Mechanical PropertiesMetricEnglishComments
    Tensile Strength, Yield 61.0 MPa8850 psiISO 527-2/50
    Elongation at Break >= 50 %>= 50 %ISO 527-2/50
    Elongation at Yield 6.0 %6.0 %ISO 527-2/50
    Tensile Modulus 2.40 GPa348 ksiISO 527-2/1
    Flexural Strength 93.0 MPa13500 psi2.0 mm/min; ISO 178
    Flexural Modulus 2.35 GPa341 ksi2.0 mm/min; ISO 178
    Charpy Impact Unnotched NBNBISO 179
    Charpy Impact, Notched 7.60 J/cm²36.2 ft-lb/in²ISO 179
     
    Electrical PropertiesMetricEnglishComments
    Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmIEC 60093
    Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmIEC 60093
    Dielectric Constant  3.0
    @Frequency 1e+6 Hz
    3.0
    @Frequency 1e+6 Hz
    IEC 60250
     3.1
    @Frequency 100 Hz
    3.1
    @Frequency 100 Hz
    IEC 60250
    Dielectric Strength 30.0 kV/mm762 kV/inshort time test; IEC 60243-1
    Dissipation Factor  0.0010
    @Frequency 100 Hz
    0.0010
    @Frequency 100 Hz
    IEC 60250
     0.0090
    @Frequency 1e+6 Hz
    0.0090
    @Frequency 1e+6 Hz
    IEC 60250
    Comparative Tracking Index 225 V225 VIEC 60112
     
    Thermal PropertiesMetricEnglishComments
    CTE, linear, Parallel to Flow 70.0 µm/m-°C38.9 µin/in-°FISO 11359-2
    CTE, linear, Transverse to Flow 70.0 µm/m-°C38.9 µin/in-°FISO 11359-2
    Deflection Temperature at 0.46 MPa (66 psi) 142 °C288 °Funannealed; ISO 75-2/B
    Deflection Temperature at 1.8 MPa (264 psi) 129 °C264 °Funannealed; ISO 75-2/A
    Vicat Softening Point 149 °C300 °FISO 306/B50
    UL RTI, Electrical 125 °C
    @Thickness 1.50 mm
    257 °F
    @Thickness 0.0591 in
    UL 746
    UL RTI, Mechanical with Impact 115 °C
    @Thickness 1.50 mm
    239 °F
    @Thickness 0.0591 in
    UL 746
    UL RTI, Mechanical without Impact 125 °C
    @Thickness 1.50 mm
    257 °F
    @Thickness 0.0591 in
    UL 746
    Flammability, UL94  V-2
    @Thickness 0.400 mm
    V-2
    @Thickness 0.0157 in
     V-2
    @Thickness 1.50 mm
    V-2
    @Thickness 0.0591 in
     V-2
    @Thickness 3.00 mm
    V-2
    @Thickness 0.118 in
    Glow Wire Ignition Temperature  850 °C
    @Thickness 1.50 mm
    1560 °F
    @Thickness 0.0591 in
    IEC 60695-2-13
     875 °C
    @Thickness 3.20 mm
    1610 °F
    @Thickness 0.126 in
    IEC 60695-2-13
    Glow Wire Flammability Index  825 °C
    @Thickness 1.50 mm
    1520 °F
    @Thickness 0.0591 in
    IEC 60695-2-12
     960 °C
    @Thickness 3.00 mm
    1760 °F
    @Thickness 0.118 in
    IEC 60695-2-12
     
    Optical PropertiesMetricEnglishComments
    Refractive Index 1.5851.585ASTM D-542
    Transmission, Visible 88 %
    @Thickness 3.00 mm
    88 %
    @Thickness 0.118 in
    ASTM D1003

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    Teijin Panlite® L-1225Z100 Weather Resistant Grade Polycarbonate
    Teijin Multilon TN-7100F Filler Reinforced Type, Halogen-Free Flame Resistant PC/ABS Polymer Alloy
    Teijin Panlite® L-1225ZL100 Transparent and Weather Resistant grade Polycarbonate Resin
    Teijin Panlite® L-1250Z100 Transparent and Weather Resistant grade Polycarbonate Resin
    Teijin Multilon T-2711 Standard, Automobile Part Series PC/ABS Polymer Alloy

    PTEIJ12 / 69701

    Aluminum Castings

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.