MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
American Basswood Wood
Categories: Wood and Natural Products; Wood; Hardwood

Material Notes: Hardwood. Easy to work with hand tools. Fair planing, poor shaping, poor steam bending. Data is based on small, clear, air-dried samples unless specified.
Usual surface texture: Fine
Dimensional changes when dried lumber is subjected to variations in humidity during service: Medium
Resistance to fungal decay (Heartwood in ground contact): Non-durable (5 to 10 years)
Resistance to penetration by preservatives: Permeable
Common Applications: Constructional veneer, turnery, piano keys, woodware

Property values marked by an asterisk (*) have been taken from an unusually old reference source.

Key Words: Tilia americana; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.320 g/ccOven Dry Weight/Unseasoned Volume
 41.0 lb/ft³Unseasoned*
 
Mechanical PropertiesOriginal ValueComments
Hardness, Wood Indentation 1100 NSide. Force required to imbed a 0.444 inch steel ball to one-half its diameter
 1200 NEnd. Force required to imbed a 0.444 inch steel ball to one-half its diameter
 1800 NSide
Tensile Strength, Ultimate 2.40 MPaPerpendicular to Grain
 280 psiPerpendicular to Grain*
Modulus of Rupture 0.0600 GPaIn Bending
 5.00 ksiStatic Bending*
Flexural Yield Strength 40.7 MPaBending stress at proportional limit
 2700 psiFiber Stress at Elastic Limit; Static Bending*
Flexural Modulus 10.1 - 10.3 GPaIn Bending
 1030 ksiStatic Bending*
Compressive Strength 2.60 MPaPerpendicular to Grain
 32.4 - 33.0 MPaParallel to Grain
 210 psiPerpendicular to Grain*
 1710 psiParallel to Grain*
 2210 psiMax Crushing Strength Parallel to Grain*
Poissons Ratio 0.022µTL, 12% Moisture Content
 0.034µRL, 12% Moisture Content
 0.346µTR, 12% Moisture Content
 0.364µLR, 12% Moisture Content
 0.406µLT, 12% Moisture Content
 0.912µRT, 12% Moisture Content
Machinability 100 %Good Relative to Other Wood
Shear Strength 6.80 MPaOrientation Unknown
 610 psiParallel to Grain*
Impact 2.0in-lb/in³; Work to Elastic Limit; Unseasoned Sample; Impact Bending*
 6200psi; Fiber Stress at Elastic Limit; Unseasoned Sample; Impact Bending*
Work to Elastic Limit 0.420 in-lb/in³Static Bending*
Work to Maximum Load 5.20 in-lb/in³Static Bending*
Cleavage 23.0 kN/mRadial surface of failure, Unseasoned*
 29.0 kN/mTangential surface of failure, Unseasoned*
 
Thermal PropertiesOriginal ValueComments
Thermal Conductivity 0.640 BTU-in/hr-ft²-°FOven Dry
 0.770 BTU-in/hr-ft²-°F12% Moisture Content
Shrinkage 6.6 %Radial; Green to Zero Moisture
 9.3 %Tangential; Green to Zero Moisture
 15.8 %Volumetric; Green to Zero Moisture
 
Descriptive Properties
ColorCreamy white to pale brownUsual for heartwood

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BCC Products MB 1300 Polyurethane Foam Modeling Board
Overview of materials for Polyetheretherketone, Carbon Fiber Filled
American Balsa Wood
DIAB ProBalsa® PB Standard Balsa Wood
American Beech Wood

PTSAN / 71297

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.