MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Proto3000 – 3D Engineering Solutions

AISI 316 Stainless Steel, Austenitic
Categories: Metal; Ferrous Metal; Stainless Steel; Cast Stainless Steel; T 300 Series Stainless Steel

Material Notes: 18Cr-12Ni-Mo STAINLESS STEEL BARS FOR GENERAL APPLICATION (SUS 316-B)

Creep and rupture data provided by NIMS

Key Words: UNS S31600; JIS G4303(91) SUS 316-B
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.03 g/cc0.290 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 187187
Tensile Strength, Ultimate 520 MPa75400 psi
Tensile Strength, Yield 205 MPa29700 psi
Elongation at Break 40 %40 %
Rupture Strength  21.0 - 22.0 MPa
@Temperature 750 °C,
Time 3.60e+8 sec
3050 - 3190 psi
@Temperature 1380 °F,
Time 100000 hour
 21.0 - 28.0 MPa
@Temperature 725 °C,
Time 3.60e+8 sec
3050 - 4060 psi
@Temperature 1340 °F,
Time 100000 hour
 27.0 - 37.0 MPa
@Temperature 700 °C,
Time 3.60e+8 sec
3920 - 5370 psi
@Temperature 1290 °F,
Time 100000 hour
 35.0 - 49.0 MPa
@Temperature 675 °C,
Time 3.60e+8 sec
5080 - 7110 psi
@Temperature 1250 °F,
Time 100000 hour
 46.0 - 65.0 MPa
@Temperature 650 °C,
Time 3.60e+8 sec
6670 - 9430 psi
@Temperature 1200 °F,
Time 100000 hour
 66.0 - 85.0 MPa
@Temperature 625 °C,
Time 3.60e+8 sec
9570 - 12300 psi
@Temperature 1160 °F,
Time 100000 hour
 97.0 - 114 MPa
@Temperature 600 °C,
Time 3.60e+8 sec
14100 - 16500 psi
@Temperature 1110 °F,
Time 100000 hour
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.080 %<= 0.080 %
Chromium, Cr 16 - 18 %16 - 18 %
Iron, Fe 61.845 - 72 %61.845 - 72 %
Manganese, Mn <= 2.0 %<= 2.0 %
Molybdenum, Mo 2.0 - 3.0 %2.0 - 3.0 %
Nickel, Ni 10 - 14 %10 - 14 %
Phosphorus, P <= 0.045 %<= 0.045 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
316 Stainless Steel, annealed bar
316 Stainless Steel, annealed sheet
AK Steel 316 Austenitic Stainless steel
304 Stainless Steel
316 Stainless Steel, annealed plate

NIMS023 / 77540

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.