MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Chosun Refractories SFC-90W High-Alumina Castable
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes:

Information provided by Chosun Refractories via Korea Institute of Ceramic Engineering and Technology (KICET).

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Modulus of Rupture 0.017658 GPa
@Temperature 110 °C,
Time 86400 sec
 0.023544 GPa
@Temperature 1000 °C,
Time 10800 sec
 0.024525 GPa
@Temperature 1400 °C,
Time 10800 sec
Compressive Strength 1000 kg(f)/cm²
@Treatment Temp. 110 °C,
Time 86400 sec
Cold Crushing Strength
 1100 kg(f)/cm²
@Treatment Temp. 1000 °C,
Time 10800 sec
Cold Crushing Strength
 1150 kg(f)/cm²
@Treatment Temp. 1400 °C,
Time 10800 sec
Cold Crushing Strength
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 1800 °Climited
Shrinkage -0.350 %
@Temperature 1400 °C,
Time 10800 sec
 -0.100 %
@Temperature 1000 °C,
Time 10800 sec
 -0.0300 %
@Temperature 110 °C,
Time 86400 sec
 
Component Elements PropertiesOriginal ValueComments
Al2O3 95 %
SiO2 4.0 %
 
Descriptive Properties
Installation MethodSelf Flowing
Material Required for Estimating (kg/m3)3,200
Water Required for Casting(%)5-5.5

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chosun Refractories HACT-180 High Alumina Castables
Chosun Refractories HACT-150 High Alumina Castables
China-Yixing Longly Refractories 95 Alumina Ceramic
Zircar Ceramics ZIRALCAST 95 Alumina Refractory Castable
Chosun Refractories SFC-90SC High-Alumina Castable

CCHOS187 / 124131

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.