Envalior Stanyl® TW241F12 PA46-GF60, Dry, 60% Glass Filled, Heat Stabilized
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 46 (PA46)
;
Nylon 46, Glass Fiber Reinforced
Material Notes:
60% Glass Reinforced, Heat Stabilized, Good Flow
Former DSM Engineering Plastics product line is now with Envalior.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.76
g/cc
0.0636
lb/in³
ISO 1183
Moisture Absorption
1.40 %
1.40 %
Humidity; Sim. ISO 62
Linear Mold Shrinkage, Flow
0.0040
cm/cm
0.0040
in/in
ISO 294-4
Linear Mold Shrinkage, Transverse
0.0070
cm/cm
0.0070
in/in
ISO 294-4
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
255
MPa
37000
psi
ISO 527-1/-2
100
MPa
@Temperature 200 °C
14500
psi
@Temperature 392 °F
ISO 527-1/-2
110
MPa
@Temperature 180 °C
16000
psi
@Temperature 356 °F
ISO 527-1/-2
125
MPa
@Temperature 160 °C
18100
psi
@Temperature 320 °F
ISO 527-1/-2
150
MPa
@Temperature 120 °C
21800
psi
@Temperature 248 °F
ISO 527-1/-2
Elongation at Break
2.0 %
2.0 %
ISO 527-1/-2
3.0 %
@Temperature 120 °C
3.0 %
@Temperature 248 °F
ISO 527-1/-2
3.0 %
@Temperature 160 °C
3.0 %
@Temperature 320 °F
ISO 527-1/-2
3.0 %
@Temperature 180 °C
3.0 %
@Temperature 356 °F
ISO 527-1/-2
3.0 %
@Temperature 200 °C
3.0 %
@Temperature 392 °F
ISO 527-1/-2
Tensile Modulus
20.0
GPa
2900
ksi
ISO 527-1/-2
8.00
GPa
@Temperature 200 °C
1160
ksi
@Temperature 392 °F
ISO 527-1/-2
8.50
GPa
@Temperature 180 °C
1230
ksi
@Temperature 356 °F
ISO 527-1/-2
9.10
GPa
@Temperature 160 °C
1320
ksi
@Temperature 320 °F
ISO 527-1/-2
10.0
GPa
@Temperature 120 °C
1450
ksi
@Temperature 248 °F
ISO 527-1/-2
Flexural Modulus
17.0
GPa
2470
ksi
ISO 178
Izod Impact, Notched (ISO)
18.0
kJ/m²
@Temperature 23.0 °C
8.57
ft-lb/in²
@Temperature 73.4 °F
ISO 180/1A
18.0
kJ/m²
@Temperature -40.0 °C
8.57
ft-lb/in²
@Temperature -40.0 °F
ISO 180/1A
Charpy Impact Unnotched
6.50
J/cm²
@Temperature -30.0 °C
30.9
ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
9.00
J/cm²
@Temperature 23.0 °C
42.8
ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched
1.80
J/cm²
@Temperature 23.0 °C
8.57
ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
1.80
J/cm²
@Temperature -30.0 °C
8.57
ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
20.0
µm/m-°C
11.1
µin/in-°F
ISO 11359-1/-2
CTE, linear, Transverse to Flow
35.0
µm/m-°C
19.4
µin/in-°F
ISO 11359-1/-2
Melting Point
295
°C
563
°F
10°C/min; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi)
290
°C
554
°F
ISO 72-1/-2
Flammability, UL94
HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
IEC 60695-11-10
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
EMS-Grivory Grivory® GV-5H PA*-GF50
Envalior Arnite® TZ6 280 PBT-(GF+GB)40, 20/20% Glass/Glass Beads Filled
Envalior Stanyl® 46HF5040 PA46-GF40 FR(17), Dry, 40% Glass Filled, Heat Stabilized, Flame Retardant
Envalior Stanyl® TW278F10 (PA46+PTFE)-GF50, Dry, 50% Glass Filled
Envalior Arnite® TV4 230 PBT-15% Glass Reinforced (European and Asian Grade)
PDSM8243 / 184944
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.