MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Hexcel® HexPly® M91/34%/UD194/IM7-12K Epoxy Matrix, IM7 Carbon Fiber
Categories: Polymer; Thermoset; Epoxy; Epoxy/Carbon Fiber Composite

Material Notes:

Information provided by Hexcel Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.28 g/cc0.0462 lb/in³Resin
 1.57 g/cc0.0567 lb/in³Theoretical Calculated Laminate
 1.78 g/cc0.0643 lb/in³Fiber
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 505 MPa73200 psi(25/50/25) (gross section); ASTM D5766
 2980 MPa432000 psiASTM D3039
Tensile Modulus 165 GPa23900 ksiASTM D3039
Compressive Strength 1860 MPa270000 psiASTM D695
Compressive Modulus 0.150 GPa21.8 ksiASTM D695
Shear Strength 110 MPa16000 psiInterlaminar; EN 2563
 315 MPa45700 psiOpen Hole, (25/50/25) (gross section); ASTM D6484
 
Thermal PropertiesMetricEnglishComments
Glass Transition Temp, Tg 185 - 190 °C365 - 374 °FDMA extrapolated onset E’; EN 6032
 
Descriptive Properties
Fabric Weight194 g/m2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHEXCB9172 / 322328

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.