MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Rhodium, Rh; As-Plated
Categories: Metal; Nonferrous Metal; Precious Metal; Pure Element

Material Notes: As-plated applies only to tensile and/or hardness values; other property values are typical of the element.

MatWeb also has entries for two other pure Rh entries.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 12.4 g/cc
 
Chemical PropertiesOriginal ValueComments
Atomic Mass 102.905501995
Atomic Number 45
Thermal Neutron Cross Section 2.6 barns/atom
X-ray Absorption Edge 0.533 ÅK
 3.64159 ÅLI
 3.94902 ÅLII
 4.13889 ÅLIII
Electrode Potential 0.80 V
Electronegativity 2.28Pauling
Ionic Radius 0.680 ÅCrystal Ionic Radius for Valence +3
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 722Converted from Vickers for 3000 kg load/10 mm ball Brinell test.
Hardness, Rockwell A 83Converted from Vickers.
Hardness, Rockwell C 63Converted from Vickers.
Hardness, Vickers 800
Tensile Strength, Ultimate 700 MPa
Modulus of Elasticity 359 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000430 ohm-cm
Magnetic Susceptibility 0.00000114cgs/g
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 21.8 J/g
Heat of Vaporization 532 J/g
CTE, linear 8.50 µm/m-°C
@Temperature 20.0 - 100 °C
Specific Heat Capacity 0.243 J/g-°C
Thermal Conductivity 151 W/m-K
Melting Point 1960 °C
Boiling Point 3695 °C
 
Optical PropertiesOriginal ValueComments
Emissivity (0-1) 0.2465 microns
Reflection Coefficient, Visible (0-1) 0.75500 nm
 
Component Elements PropertiesOriginal ValueComments
Rhodium, Rh 100 %
 
Descriptive Properties
CAS Number7440-16-6

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Rhodium, Rh; Annealed
Rhodium, Rh; Hardened
Silver, Ag
Ruthenium, Ru; Annealed
Ruthenium, Ru; Hot Rolled Bar

AMERh01 / 94

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.