MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Titanium Beta C (Ti-3Al-8V-6Cr-4Mo-4Zr) Solution Treated 815°C
Categories: Metal; Nonferrous Metal; Titanium Alloy; Beta Titanium Alloy

Material Notes: Equiaxed beta grain structure (bcc). Highly formable, able to be cold-worked, better corrosion properties than other high strength alloys

Applications: Fasteners, springs, torsion bars, foil.

3 other heat treatments of this alloy are in MatWeb.

Key Words: Ti-38-6-44; UNS R58640; Ti-3Al-8V-6Cr-4Mo-4Zr; TIMETAL 3-8-6-44
Vendors:
TITANIUM ENGINEERS is your source for high strength, NACE titanium alloys, with a full range of stock sizes and sizes made to order. Our in-house metallurgical experts ensure the best alloy selection and process titanium to meet unique customer specifications. Please visit our website www.TitaniumEngineers.com for more information or call us at +1 281 265 2910 (USA) or +44 (0) 1675 464200 (UK).

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 4.82 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 304Estimated from Rockwell C.
Hardness, Knoop 330Estimated from Rockwell C.
Hardness, Rockwell C 32
Hardness, Vickers 318Estimated from Rockwell C.
Tensile Strength, Ultimate 860 MPa
Tensile Strength, Yield 825 MPa
Elongation at Break 7.0 %
Modulus of Elasticity 88.0 GPa
Poissons Ratio 0.33After ST 815ºC, Aged 510ºC
Shear Modulus 40.0 GPaAged
Shear Strength 620 MPaUltimate shear strength
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000160 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 8.30 µm/m-°C
@Temperature 20.0 - 100 °C
 8.70 µm/m-°C
@Temperature 20.0 - 250 °C
estimated from lower temperatures
Specific Heat Capacity 0.515 J/g-°C
Thermal Conductivity 6.20 W/m-K
Melting Point 1555 - 1650 °C
Solidus 1555 °C
Liquidus 1650 °C
Beta Transus 730 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 3.0 %
Carbon, C <= 0.050 %
Chromium, Cr 6.0 %
Iron, Fe <= 0.30 %
Molybdenum, Mo 4.0 %
Nitrogen, N <= 0.030 %
Oxygen, O <= 0.14 %
Titanium, Ti 75 %
Vanadium, V 8.0 %
Zirconium, Zr 4.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Titanium Beta C (Ti-3Al-8V-6Cr-4Mo-4Zr ST 815°C, Aged 510°C
Titanium Beta C (Ti-3Al-8V-6Cr-4Mo-4Zr ST 815°C, Aged 565°C
Titanium Beta C (Ti-3Al-8V-6Cr-4Mo-4Zr ST 815°C, Aged 425°C
Titanium Ti-6Al-4V (Grade 5), Annealed
Titanium Grade 19 Ti-3Al-8V-6Cr-4Mo-4Zr

MTB0C0 / 14158

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.