MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Avient Nymax™ GF 1200 A 55 HS Black 13 Polyamide 66 (Nylon 66)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66)

Material Notes: The Nymax® GF 1200 Series of glass fiber-reinforced nylon 6/6 compounds have been specifically formulated for applications requiring high stiffness, tensile properties, heat resistance, and durability in harsh environments. These materials are available in a broad range of reinforcement levels depending upon stiffness characteristics desired and have been formulated to offer ease of processing in most standard thermoplastic processing equipment

Molded Test Bars: Dry as Molded

Information provided by PolyOne

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.60 g/ccASTM D792
Filler Content 55 %Unspecified
Water Absorption 0.60 %
@Thickness 3.18 mm
@ 24 hrs; ASTM D570
Linear Mold Shrinkage, Flow 0.0010 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 193 MPaType I, 5.1 mm/min; ASTM D638
Tensile Strength 215 MPa5.0 mm/min; ISO 527
Elongation at Break 2.5 %Type I, 5.1 mm/min; ASTM D638
Flexural Strength 310 MPaASTM D790
Flexural Modulus 15200 MPaASTM D790
 15500 MPa25 mm/min; ISO 178
Izod Impact, Notched 140 J/m
@Thickness 3.18 mm,
Temperature 23.0 °C
Injection Molded; ASTM D256A
Izod Impact, Notched (ISO) 12.0 kJ/m²ISO 180
 
Thermal PropertiesOriginal ValueComments
Melting Point 260 °CASTM D789
Deflection Temperature at 0.46 MPa (66 psi) 257 °C
@Thickness 3.18 mm
Unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 248 °CUnannealed; ISO 75-2
 255 °C
@Thickness 3.18 mm
Unannealed; ASTM D648
 
Processing PropertiesOriginal ValueComments
Mold Temperature 60.0 - 107 °C
Drying Temperature 82.2 °C
Dry Time 4.00 hour
 
Descriptive Properties
AdditiveHeat Stabilizer
AppearanceBlack
FeaturesHeat Stabilized
Filler / ReinforcementGlass Fiber Reinforcement
FormsPellets
Generic MaterialNylon 66
Generic NamePolyamide 66 (Nylon 66)
Regional AvailabilityNorth America
 South America

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Stratasys® FDM Nylon 12™ 3D Printing Polymer; Dry
Stratasys® FDM Nylon 12™ 3D Printing Polymer; Conditioned
Celanese Celstran® PA66-GF50-02-US Nylon 66, 50% Glass Reinforced
Avient Nymax™ GF 1200 A 13 Black 13 Polyamide 66 (Nylon 66)

PH0POL0362 / 144931

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.