MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Alclad Aluminum 6061-T4, T451
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 6000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes: Composition for AA 6061 (not Alclad 6061 specifically).
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A86061; al6061, Alclad 6061-T4, T451; Alclad 6061-T4, T451; Al6061-T4
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 2.70 g/ccFor AA6061 (Not Alclad)
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 33.0 ksiAA; Typical
Tensile Strength, Yield 19.0 ksiAA; Typical
Elongation at Break 22 %
@Thickness 1.59 mm
AA; Typical
Modulus of Elasticity 10000 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Shear Strength 22.0 ksiAA; Typical
 
Processing PropertiesOriginal ValueComments
Solution Temperature 985 °F
Aging Temperature 320 °FRolled or drawn products; hold at temperature for 18 hr
 350 °FExtrusions or forgings; hold at temperature for 8 hr
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 95.8 - 98.6 %As remainder
Chromium, Cr 0.04 - 0.35 %
Copper, Cu 0.15 - 0.40 %
Iron, Fe <= 0.70 %
Magnesium, Mg 0.80 - 1.2 %
Manganese, Mn <= 0.15 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si 0.40 - 0.80 %
Titanium, Ti <= 0.15 %
Zinc, Zn <= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Alclad Aluminum 6061-T6, T651
Aluminum 6061-T4; 6061-T451
Alclad Aluminum 6061-O
Aluminum 6061-T6; 6061-T651
Aluminum 6061-O

MA6061AT4 / 9387

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.