MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Erbslöh Aluminium DISPAL S270 Aluminum Alloy, AlSi25Fe4Ni3CuMgMnCrTi, Condition T4
Categories: Metal; Nonferrous Metal; Aluminum Alloy

Material Notes: Excellent properties:
  • abrasive stability
  • high stiffness (E-modulus)
  • resistance even at high temperatures
  • good grindability

PEAK DISPAL materials allow the manufacturing of pistons for highest operational demands.

Information provided by PEAK Werkstoff GmbH, a part of Erbslöh Aluminium GmbH.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.651 - 2.930 g/cc0.09576 - 0.1058 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers >= 175>= 175HV30, Condition T4 (Quenching in water at 80)
 >= 180>= 180HV30, Condition T4 (Quenching in water at RT)
Tensile Strength at Break  >= 385 MPa
@Temperature 20.0 °C
>= 55800 psi
@Temperature 68.0 °F
Condition T4 (Quenching in water at 80C)
 >= 439 MPa
@Temperature 20.0 °C
>= 63700 psi
@Temperature 68.0 °F
Condition T4 (Quenching in water at RT)
Tensile Strength, Yield  >= 279 MPa
@Temperature 20.0 °C
>= 40500 psi
@Temperature 68.0 °F
Condition T4 (Quenching in water at 80C)
 >= 335 MPa
@Temperature 20.0 °C
>= 48600 psi
@Temperature 68.0 °F
Condition T4 (Quenching in water at RT)
Elongation at Break  >= 0.30 %
@Temperature 20.0 °C
>= 0.30 %
@Temperature 68.0 °F
Condition T4 (Quenching in water at RT)
 >= 0.70 %
@Temperature 20.0 °C
>= 0.70 %
@Temperature 68.0 °F
Condition T4 (Quenching in water at 80C)
Modulus of Elasticity  >= 96.0 GPa
@Temperature 20.0 °C
>= 13900 ksi
@Temperature 68.0 °F
Condition T4 (Quenching in water at 80C)
 >= 98.0 GPa
@Temperature 20.0 °C
>= 14200 ksi
@Temperature 68.0 °F
Condition T4 (Quenching in water at RT)
Poissons Ratio  0.284
@Temperature 20.0 °C
0.284
@Temperature 68.0 °F
Condition F
 0.286
@Temperature 100 °C
0.286
@Temperature 212 °F
Condition F
 0.288
@Temperature 150 °C
0.288
@Temperature 302 °F
Condition F
 0.289
@Temperature 200 °C
0.289
@Temperature 392 °F
Condition F
 0.291
@Temperature 250 °C
0.291
@Temperature 482 °F
Condition F
 0.292
@Temperature 300 °C
0.292
@Temperature 572 °F
Condition F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000940 - 0.0000104 ohm-cm0.00000940 - 0.0000104 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  15.2 - 16.2 µm/m-°C
@Temperature 20.0 - 100 °C
8.44 - 9.00 µin/in-°F
@Temperature 68.0 - 212 °F
 15.7 - 16.7 µm/m-°C
@Temperature 20.0 - 200 °C
8.72 - 9.28 µin/in-°F
@Temperature 68.0 - 392 °F
 16.3 - 17.3 µm/m-°C
@Temperature 20.0 - 300 °C
9.06 - 9.61 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.800 - 0.840 J/g-°C0.191 - 0.201 BTU/lb-°F
Thermal Conductivity  89.60 W/m-K
@Temperature 400 °C
621.8 BTU-in/hr-ft²-°F
@Temperature 752 °F
 93.70 W/m-K
@Temperature 300 °C
650.3 BTU-in/hr-ft²-°F
@Temperature 572 °F
 94.90 W/m-K
@Temperature 200 °C
658.6 BTU-in/hr-ft²-°F
@Temperature 392 °F
 96.30 W/m-K
@Temperature 100 °C
668.3 BTU-in/hr-ft²-°F
@Temperature 212 °F
 98.40 W/m-K
@Temperature 30.0 °C
682.9 BTU-in/hr-ft²-°F
@Temperature 86.0 °F
Melting Point 536 - 777 °C997 - 1430 °F
Solidus 536.3 - 542.3 °C997.3 - 1008 °F
Liquidus 770.9 - 776.9 °C1420 - 1430 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 63 %63 %As Balance
Chromium, Cr 1.0 %1.0 %
Copper, Cu 1.0 %1.0 %
Iron, Fe 4.0 %4.0 %
Magnesium, Mg 1.0 %1.0 %
Manganese, Mn 1.0 %1.0 %
Nickel, Ni 3.0 %3.0 %
Silicon, Si 25 %25 %
Titanium, Ti 1.0 %1.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Erbslöh Aluminium DISPAL S250 Aluminum Alloy, AlSi20Fe5Ni2, Condition F
Erbslöh Aluminium DISPAL S270 Aluminum Alloy, AlSi25Fe4Ni3CuMgMnCrTi, Condition T6
Erbslöh Aluminium DISPAL S270 Aluminum Alloy, AlSi25Fe4Ni3CuMgMnCrTi, Condition F
Erbslöh Aluminium DISPAL S220 Aluminum Alloy, AlSi35, Condition O
Erbslöh Aluminium DISPAL S226 Aluminum Alloy, AlSi30CuMg, Condition T6

NPEAK06ba / 170258

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.