MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Akro-Plastic Akromid® C3 GF 30 1 black (4363) PA 6.6/6 Conditioned, Heat Stabilized
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6/66; Nylon 66/6, 30% Glass Fiber Reinforced

Material Notes: Description: AKROMID C3 GF 30 1 black (4363) is a 30% glass fiber reinforced, heat stabilized polyamide 6.6/6 – Blend. Applications are mainly components in mechanical engineering and the automotive industry where good flowability is required.

Additive: Heat Stabilizer

Features:

  • Good Flow
  • Heat Stability
Uses:
  • Automotive Applications
  • Engineering Parts

Information provided by Akro-Plastic GmbH

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.36 g/cc0.0491 lb/in³ISO 1183
Filler Content 30 %30 %ISO 1172
Moisture Absorption 1.9 %
@Temperature 70.0 °C
1.9 %
@Temperature 158 °F
Humidity, 62% RH; ISO 1110
Linear Mold Shrinkage, Flow 0.0030 cm/cm0.0030 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.0090 cm/cm0.0090 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 120 MPa17400 psi5 [mm/min]; ISO 527-2
Elongation at Break 5.5 %5.5 %5 [mm/min]; ISO 527-2
Tensile Modulus 6.50 GPa943 ksi1 [mm/min]; ISO 527-2
Charpy Impact Unnotched 9.00 J/cm²
@Temperature 23.0 °C
42.8 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched 1.40 J/cm²
@Temperature 23.0 °C
6.66 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 260 °C500 °FDIN EN 11357-1
 
Descriptive Properties
Resistant to Carbon tetrachloridePass100% Conc. at 23°C
Resistant to Citric acidPass10% Conc. at 23°C
Resistant to Ethyl acetatePass100% Conc. at 23°C
Resistant to Hydrochloric acidFail36% Conc. at 23°C
Resistant to Hydrogen peroxideFail23°C
Resistant to SeawaterPass100% Conc. at 23°C
Resistant to Silicone fluidPass23°C
Resistant to Sodium hypochlorite, aqueousFail5% Conc. at 23°C
Resistant to Sulfuric acidFail10% Conc. at 23°C
Resistant to Super-grade petrol (DIN 51600)Pass100% Conc. at 23°C
Resistant to ToluolPass100% Conc. at 23°C
Resistant to WaterPass100% Conc. up to 50°C
Resistant to XylolPass100% Conc. at 23°C
Resistant to Zinc chloride, aqueousFail50% Conc. at 23°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Akro-Plastic Akromid® C3 1 (4546) PA66/6 Conditioned
Akro-Plastic Akromid® C3 GF 30 5 XTC (4499) PA66/6 Conditioned, 30% Glass Filled
Celanese Zytel® 74G33W BK196 PA66+PA6-GF33
Domo TECHNYL® A 218 V30 Black 21 NS PA 66 30% Glass Reinforced, Conditioned
EMS-Grivory Grilon® TSG-30 PA666-GF30

PAKRO351 / 182938

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.