MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Overview of materials for Polypropylene Copolymer
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene Copolymer

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polypropylene Copolymer". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.780 - 2.77 g/cc0.0282 - 0.100 lb/in³Average value: 0.948 g/cc Grade Count:1422
Filler Content 0.000 - 75.0 %0.000 - 75.0 %Average value: 22.7 % Grade Count:90
Water Absorption 0.0100 - 0.200 %0.0100 - 0.200 %Average value: 0.0195 % Grade Count:151
Moisture Absorption at Equilibrium 0.100 %0.100 %Average value: 0.100 % Grade Count:3
Water Absorption at Saturation 0.100 - 0.900 %0.100 - 0.900 %Average value: 0.367 % Grade Count:3
Water Vapor Transmission 18.8 - 18.8 g/m²/day
@Temperature 37.8 - 37.8 °C
1.21 - 1.21 g/100 in²/day
@Temperature 100 - 100 °F
Average value: 18.8 g/m²/day Grade Count:1
Oxidative Induction Time (OIT) 40.0 min40.0 minAverage value: 40.0 min Grade Count:3
 20.0 - 40.0 min
@Temperature 190 - 220 °C
20.0 - 40.0 min
@Temperature 374 - 428 °F
Average value: 42.5 min Grade Count:8
Maximum Moisture Content 0.0200 - 0.2000.0200 - 0.200Average value: 0.0650 Grade Count:4
Thickness 1570 - 250000 microns62.0 - 9840 milAverage value: 30400 microns Grade Count:96
Linear Mold Shrinkage 0.000150 - 0.0350 cm/cm0.000150 - 0.0350 in/inAverage value: 0.0128 cm/cm Grade Count:284
 0.00800 - 0.00900 cm/cm
@Temperature 80.0 - 80.0 °C
0.00800 - 0.00900 in/in
@Temperature 176 - 176 °F
Average value: 0.00850 cm/cm Grade Count:2
Linear Mold Shrinkage, Transverse 0.00400 - 0.0250 cm/cm0.00400 - 0.0250 in/inAverage value: 0.0126 cm/cm Grade Count:78
 0.00900 - 0.0100 cm/cm
@Temperature 80.0 - 80.0 °C
0.00900 - 0.0100 in/in
@Temperature 176 - 176 °F
Average value: 0.00950 cm/cm Grade Count:2
Melt Flow 0.200 - 150 g/10 min0.200 - 150 g/10 minAverage value: 19.1 g/10 min Grade Count:1501
Base Resin Melt Index 1.20 - 45.0 g/10 min
@Temperature 230 - 230 °C
1.20 - 45.0 g/10 min
@Temperature 446 - 446 °F
Average value: 16.4 g/10 min Grade Count:23
Ash 0.000 - 40.0 %0.000 - 40.0 %Average value: 15.3 % Grade Count:35
 0.300 - 5.00 %
@Temperature 600 - 900 °C
0.300 - 5.00 %
@Temperature 1110 - 1650 °F
Average value: 3.48 % Grade Count:9
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 55.0 - 80.055.0 - 80.0Average value: 61.3 Grade Count:4
Hardness, Rockwell R 33.0 - 11233.0 - 112Average value: 86.9 Grade Count:449
Hardness, Shore D 48.0 - 85.048.0 - 85.0Average value: 67.8 Grade Count:244
Ball Indentation Hardness 35.0 - 82.0 MPa5080 - 11900 psiAverage value: 60.0 MPa Grade Count:27
Tensile Strength, Ultimate 5.00 - 128 MPa725 - 18500 psiAverage value: 27.6 MPa Grade Count:320
 9.00 - 15.0 MPa
@Temperature 60.0 - 90.0 °C
1310 - 2180 psi
@Temperature 140 - 194 °F
Average value: 12.0 MPa Grade Count:1
Film Tensile Strength at Yield, MD 18.0 - 27.0 MPa2610 - 3920 psiAverage value: 20.4 MPa Grade Count:8
Tensile Strength, Yield 8.48 - 110 MPa1230 - 16000 psiAverage value: 25.8 MPa Grade Count:1299
Film Elongation at Break, MD 80.0 - 800 %80.0 - 800 %Average value: 602 % Grade Count:27
Film Elongation at Break, TD 50.0 - 800 %50.0 - 800 %Average value: 576 % Grade Count:13
Film Elongation at Yield, MD 9.00 - 17.0 %9.00 - 17.0 %Average value: 12.0 % Grade Count:3
Elongation at Break 1.30 - 1000 %1.30 - 1000 %Average value: 230 % Grade Count:514
 6.00 - 100 %
@Temperature -30.0 - -17.7 °C
6.00 - 100 %
@Temperature -22.0 - 0.126 °F
Average value: 18.2 % Grade Count:14
Elongation at Yield 0.500 - 500 %0.500 - 500 %Average value: 15.5 % Grade Count:748
Modulus of Elasticity 0.0340 - 6.20 GPa4.93 - 899 ksiAverage value: 1.29 GPa Grade Count:278
Flexural Yield Strength 13.4 - 181 MPa1950 - 26300 psiAverage value: 48.7 MPa Grade Count:176
Flexural Modulus 0.0150 - 9.32 GPa2.18 - 1350 ksiAverage value: 1.37 GPa Grade Count:1438
 0.370 - 0.560 GPa
@Temperature 60.0 - 90.0 °C
53.7 - 81.2 ksi
@Temperature 140 - 194 °F
Average value: 0.465 GPa Grade Count:1
Compressive Yield Strength 27.6 - 110 MPa4000 - 16000 psiAverage value: 42.5 MPa Grade Count:7
Shear Modulus 0.260 - 0.730 GPa37.7 - 106 ksiAverage value: 0.541 GPa Grade Count:20
Secant Modulus 0.345 - 1.60 GPa50.0 - 232 ksiAverage value: 1.09 GPa Grade Count:18
Secant Modulus, MD 0.370 - 0.840 GPa53.7 - 122 ksiAverage value: 0.632 GPa Grade Count:5
Izod Impact, Notched 0.196 J/cm - NB0.367 ft-lb/in - NBAverage value: 1.52 J/cm Grade Count:1011
 0.160 - 99.99 J/cm
@Temperature -40.0 - 3.89 °C
0.300 - 187.3 ft-lb/in
@Temperature -40.0 - 39.0 °F
Average value: 0.780 J/cm Grade Count:144
 0.200 J/cm - NB
@Temperature -30.0 - 0.000 °C
0.375 ft-lb/in - NB
@Temperature -22.0 - 32.0 °F
Average value: 0.780 J/cm Grade Count:26
 0.200 J/cm - NB
@Thickness 3.17 - 3.17 mm
0.375 ft-lb/in - NB
@Thickness 0.125 - 0.125 in
Average value: 0.780 J/cm Grade Count:26
 0.48051 - 0.5339 J/cm
@Diameter 3.00 - 3.00 mm
0.90019 - 1.000 ft-lb/in
@Diameter 0.118 - 0.118 in
Average value: 0.780 J/cm Grade Count:3
 0.48051 - 0.5339 J/cm
@Temperature -20.0 - -20.0 °C
0.90019 - 1.000 ft-lb/in
@Temperature -4.00 - -4.00 °F
Average value: 0.780 J/cm Grade Count:3
Izod Impact, Unnotched 0.294 J/cm - NB0.551 ft-lb/in - NBAverage value: 3.68 J/cm Grade Count:92
 0.294199 - 1.12119 J/cm
@Temperature -30.0 - -10.0 °C
0.551156 - 2.10045 ft-lb/in
@Temperature -22.0 - 14.0 °F
Average value: 0.655 J/cm Grade Count:24
 1.0678 - 1.0678 J/cm
@Temperature -20.0 - -20.0 °C
2.0004 - 2.0004 ft-lb/in
@Temperature -4.00 - -4.00 °F
Average value: 0.655 J/cm Grade Count:1
 1.0678 - 1.0678 J/cm
@Thickness 3.17 - 3.17 mm
2.0004 - 2.0004 ft-lb/in
@Thickness 0.125 - 0.125 in
Average value: 0.655 J/cm Grade Count:1
Izod Impact, Notched (ISO) 2.94 - 21000 kJ/m²1.40 - 9990 ft-lb/in²Average value: 20.0 kJ/m² Grade Count:208
 2.00 - 70.98 kJ/m²
@Temperature -40.0 - 4.00 °C
0.952 - 33.78 ft-lb/in²
@Temperature -40.0 - 39.2 °F
Average value: 5.74 kJ/m² Grade Count:107
Izod Impact, Unnotched (ISO) 7.10 kJ/m² - NB3.38 ft-lb/in² - NBAverage value: 47.8 kJ/m² Grade Count:14
Charpy Impact Unnotched 1.00 J/cm² - NB4.76 ft-lb/in² - NBAverage value: 5.30 J/cm² Grade Count:116
 1.20 J/cm² - NB
@Temperature -40.0 - 0.000 °C
5.71 ft-lb/in² - NB
@Temperature -40.0 - 32.0 °F
Average value: 8.44 J/cm² Grade Count:49
Charpy Impact, Notched 0.250 - 1000 J/cm²1.19 - 4760 ft-lb/in²Average value: 2.12 J/cm² Grade Count:367
 0.100 - 12.0 J/cm²
@Temperature -40.0 - 0.000 °C
0.476 - 57.1 ft-lb/in²
@Temperature -40.0 - 32.0 °F
Average value: 0.534 J/cm² Grade Count:254
Gardner Impact 1.25 - 136 J0.920 - 100 ft-lbAverage value: 23.8 J Grade Count:86
 1.00 - 36.0 J
@Temperature -30.0 - -20.0 °C
0.738 - 26.6 ft-lb
@Temperature -22.0 - -4.00 °F
Average value: 20.8 J Grade Count:49
 4.86 - 33.7825 J
@Temperature -28.9 - -20.0 °C
3.58 - 24.9167 ft-lb
@Temperature -20.0 - -4.00 °F
Average value: 20.8 J Grade Count:9
 4.86 - 33.7825 J
@Thickness 3.17 - 3.18 mm
3.58 - 24.9167 ft-lb
@Thickness 0.125 - 0.125 in
Average value: 20.8 J Grade Count:9
Dart Drop, Total Energy 5.20 - 50.0 J3.84 - 36.9 ft-lbAverage value: 23.3 J Grade Count:27
 11.0 - 38.3697 J
@Temperature -30.0 - -17.8 °C
8.11 - 28.3000 ft-lb
@Temperature -22.0 - -0.0400 °F
Average value: 25.6 J Grade Count:14
Falling Dart Impact 2.26 - 33.0 J1.67 - 24.3 ft-lbAverage value: 9.75 J Grade Count:11
 28.2011 - 28.2011 J
@Temperature -30.0 - -30.0 °C
20.8000 - 20.8000 ft-lb
@Temperature -22.0 - -22.0 °F
Average value: 13.1 J Grade Count:1
 3.00 - 27.0 J
@Temperature -30.0 - -30.0 °C
2.21 - 19.9 ft-lb
@Temperature -22.0 - -22.0 °F
Average value: 13.1 J Grade Count:5
 3.00 - 27.0 J
@Thickness 3.17 - 3.17 mm
2.21 - 19.9 ft-lb
@Thickness 0.125 - 0.125 in
Average value: 13.1 J Grade Count:5
Instrumented Impact Total Energy 3.84 - 35.0 J2.83 - 25.8 ft-lbAverage value: 24.8 J Grade Count:3
Puncture Energy 10.0 - 48.0 J
@Temperature -40.0 - 0.000 °C
7.38 - 35.4 ft-lb
@Temperature -40.0 - 32.0 °F
Average value: 23.6 J Grade Count:14
Coefficient of Friction 0.100 - 1.000.100 - 1.00Average value: 0.341 Grade Count:26
Dart Drop Total Energy 6.73 - 7.79 J/cm0.0126 - 0.0146 ft-lb/milAverage value: 7.08 J/cm Grade Count:3
Film Tensile Strength at Break, MD 21.0 - 440 MPa3050 - 63800 psiAverage value: 66.6 MPa Grade Count:35
Film Tensile Strength at Break, TD 25.0 - 340 MPa3630 - 49300 psiAverage value: 65.7 MPa Grade Count:27
Tangent Modulus 740 - 1590 MPa107000 - 230000 psiAverage value: 1150 MPa Grade Count:16
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 10.0 - 1.00e+17 ohm-cm10.0 - 1.00e+17 ohm-cmAverage value: 9.36e+15 ohm-cm Grade Count:43
Surface Resistance 80.0 - 1.00e+16 ohm80.0 - 1.00e+16 ohmAverage value: 7.17e+14 ohm Grade Count:57
Dielectric Constant 2.20 - 3.802.20 - 3.80Average value: 2.50 Grade Count:13
Dielectric Strength 11.8 - 45.0 kV/mm300 - 1140 kV/inAverage value: 29.2 kV/mm Grade Count:20
Comparative Tracking Index 450 - 650 V450 - 650 VAverage value: 591 V Grade Count:35
 
Thermal PropertiesMetricEnglishComments
CTE, linear 15.0 - 270 µm/m-°C8.33 - 150 µin/in-°FAverage value: 133 µm/m-°C Grade Count:119
Thermal Conductivity 0.130 - 2.00 W/m-K0.900 - 13.9 BTU-in/hr-ft²-°FAverage value: 0.398 W/m-K Grade Count:18
Melting Point 73.9 - 171 °C165 - 340 °FAverage value: 157 °C Grade Count:264
Crystallization Temperature 35.0 - 130 °C95.0 - 266 °FAverage value: 101 °C Grade Count:14
Maximum Service Temperature, Air 65.0 - 300 °C149 - 572 °FAverage value: 88.8 °C Grade Count:119
Deflection Temperature at 0.46 MPa (66 psi) 34.0 - 225 °C93.2 - 437 °FAverage value: 94.5 °C Grade Count:1058
Deflection Temperature at 1.8 MPa (264 psi) 37.0 - 165 °C98.6 - 329 °FAverage value: 65.2 °C Grade Count:474
 105 - 105 °C
@Temperature 0.250 - 0.250 °C
221 - 221 °F
@Temperature 32.5 - 32.5 °F
Average value: 105 °C Grade Count:1
Vicat Softening Point 49.0 - 189 °C120 - 372 °FAverage value: 123 °C Grade Count:360
Heat Distortion Temperature 75.0 - 83.0 °C167 - 181 °FAverage value: 79.3 °C Grade Count:6
Brittleness Temperature -70.0 - -20.0 °C-94.0 - -4.00 °FAverage value: -43.8 °C Grade Count:9
UL RTI, Electrical 48.9 - 115 °C120 - 239 °FAverage value: 81.3 °C Grade Count:7
UL RTI, Mechanical with Impact 48.9 - 65.0 °C120 - 149 °FAverage value: 61.0 °C Grade Count:4
UL RTI, Mechanical without Impact 48.9 - 65.0 °C120 - 149 °FAverage value: 61.0 °C Grade Count:4
Flammability, UL94 HB - V-0HB - V-0Grade Count:230
Flame Spread 25.0 - 100 mm/min0.984 - 3.94 in/minAverage value: 75.4 mm/min Grade Count:6
Flash Point 340 °C644 °FAverage value: 340 °C Grade Count:10
Glow Wire Test 550 - 960 °C1020 - 1760 °FAverage value: 797 °C Grade Count:51
Ignition Temperature 350 °C662 °FAverage value: 350 °C Grade Count:6
DSC Induction Temperature 135 - 164 °C275 - 327 °FAverage value: 149 °C Grade Count:7
 
Optical PropertiesMetricEnglishComments
Haze 0.500 - 60.0 %0.500 - 60.0 %Average value: 11.8 % Grade Count:134
Gloss 3.00 - 150 %3.00 - 150 %Average value: 90.1 % Grade Count:79
Yellow Index -10.0 - -5.00 %-10.0 - -5.00 %Average value: -8.00 % Grade Count:10
Transmission, Visible 14.3 - 90.0 %14.3 - 90.0 %Average value: 80.3 % Grade Count:25
 
Processing PropertiesMetricEnglishComments
Processing Temperature 20.0 - 280 °C68.0 - 536 °FAverage value: 201 °C Grade Count:33
Nozzle Temperature 188 - 260 °C370 - 500 °FAverage value: 214 °C Grade Count:72
Die Temperature 175 - 260 °C347 - 500 °FAverage value: 213 °C Grade Count:28
Melt Temperature 145 - 302 °C293 - 575 °FAverage value: 215 °C Grade Count:262
Head Temperature 180 - 230 °C356 - 446 °FAverage value: 214 °C Grade Count:18
Mold Temperature 4.44 - 90.6 °C40.0 - 195 °FAverage value: 41.9 °C Grade Count:239
Drying Temperature 60.0 - 120 °C140 - 248 °FAverage value: 78.6 °C Grade Count:130
Moisture Content 0.0200 - 0.200 %0.0200 - 0.200 %Average value: 0.0555 % Grade Count:50
Injection Pressure 0.500 - 140 MPa72.5 - 20300 psiAverage value: 50.6 MPa Grade Count:96
 
Component Elements PropertiesMetricEnglishComments
SiO2 0.180 %0.180 %Average value: 0.180 % Grade Count:5

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polypropylene, Molded
IRPC Polimaxx Polene 2300K Polypropylene Block Copolymer
Overview of materials for Polypropylene, Extrusion Grade
Overview of materials for High Density Polyethylene (HDPE), Injection Molded
Overview of materials for Polypropylene, Impact Modified; Molded/Extruded

O4747 / 78395

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.