MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Manganese Bronze, UNS C86300, Copper Casting Alloy
Categories: Metal; Nonferrous Metal; Copper Alloy; Copper Casting Alloy

Material Notes:

Casting methods recommended for this alloy: Centrifugal, Investment, Plaster, and Sand.

Applications: Extra heavy duty, high strength alloy. Large valve stems, gears, cams, slow-speed heavy-load bearings, screwdown nuts hydraulic cylinder parts.

Classified under: Manganese and leaded manganese bronze alloys. ASTM B22; ASTM B584; formerly ASTM B22-E; ASTM B147-8C

As cast values below are for sand casting. Alloy does not respond to heat treating. Casting shrinkage allowance is 2.3%

Key Words: High Strength Manganese Bronze, ASTM B22; ASTM B584; ASTM B22-E; ASTM B147-8C
Vendors: Dura-Bar Metal Services is a major distributor of bronze alloys. We stock a large inventory of C86300 in tubes and rounds. Our customers rely on us for high quality materials that help increase their profitability. Call us at 1-800-526-0548 or visit dura-barms.com for more information.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 7.70 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 2253000 kg
Tensile Strength, Ultimate 820 MPa
Tensile Strength, Yield 460 MPa
Elongation at Break 18 %In 50 mm
Modulus of Elasticity 105 GPa
Fatigue Strength 170 MPa
@# of Cycles 1.00e+8
rotating beam
Machinability 8 %UNS C36000 (free-cutting brass) = 100%
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000192 ohm-cm
@Temperature 20.0 °C
9% IACS
Magnetic Permeability 1.09
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.0 µin/in-°F
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.0900 BTU/lb-°F
Thermal Conductivity 20.5 BTU-in/hr-ft²-°F
Melting Point 885 - 920 °C
Solidus 885 °C
Liquidus 923 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 3.0 - 7.5 %
Copper, Cu 60 - 68 %
Iron, Fe 2.0 - 4.0 %
Lead, Pb <= 0.20 %
Manganese, Mn 2.5 - 5.0 %
Tin, Sn <= 0.20 %
Zinc, Zn 25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
MetalTek C86300 High Tensile Manganese Bronze
Manganese Bronze, UNS C86200, Copper Casting Alloy
High-Strength Yellow Brass, UNS C86500, Copper Casting Alloy
Aluminum Bronze, UNS C95400, Copper Casting Alloy, As Cast
Manganese Bronze A, UNS C67500

MC86300b1 / 11914

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.