MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Aluminum 7005-T53
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 7000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A97005; Aluminium 7005-T53; AA7005-T53; Al7005-T53
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.78 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 105500 kg load with 10 mm ball. Calculated value.
Hardness, Knoop 132Converted from Brinell Hardness Value
Hardness, Rockwell A 42.9Converted from Brinell Hardness Value
Hardness, Rockwell B 66Converted from Brinell Hardness Value
Hardness, Vickers 118Converted from Brinell Hardness Value
Tensile Strength, Ultimate 390 MPa
 76.0 MPa
@Temperature 260 °C
 97.0 MPa
@Temperature 204 °C
 165 MPa
@Temperature 149 °C
 303 MPa
@Temperature 100 °C
 392 MPa
@Temperature 24.0 °C
 421 MPa
@Temperature -28.0 °C
 441 MPa
@Temperature -80.0 °C
 538 MPa
@Temperature -196 °C
 641 MPa
@Temperature -269 °C
Tensile Strength, Yield 345 MPa
 66.0 MPa
@Temperature 260 °C
 83.0 MPa
@Temperature 204 °C
 145 MPa
@Temperature 149 °C
 283 MPa
@Temperature 100 °C
 345 MPa
@Temperature 24.0 °C
 359 MPa
@Temperature -28.0 °C
 379 MPa
@Temperature -80.0 °C
 421 MPa
@Temperature -196 °C
 483 MPa
@Temperature -269 °C
Elongation at Break 15 %In 5 cm; Sample 1.6 mm thick
 13 %
@Temperature -80.0 °C
 14 %
@Temperature -28.0 °C
 15 %
@Temperature 24.0 °C
 16 %
@Temperature -269 °C
 16 %
@Temperature -196 °C
 20 %
@Temperature 100 °C
 35 %
@Temperature 149 °C
 60 %
@Temperature 204 °C
 80 %
@Temperature 260 °C
Modulus of Elasticity 72.0 GPaAverage of Tension and Compression. In Al alloys, the compressive modulus is typically 2% greater than the tensile modulus
Poissons Ratio 0.33Estimated from trends in similar Al alloys.
Fatigue Strength 140 MPa
@# of Cycles 5.00e+8
Shear Modulus 26.9 GPa
Shear Strength 300 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000450 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 21.4 µm/m-°C
@Temperature -50.0 - 20.0 °C
 23.1 µm/m-°C
@Temperature 20.0 - 100 °C
 23.6 µm/m-°C
@Temperature 20.0 - 100 °C
 24.0 µm/m-°C
@Temperature 20.0 - 200 °C
 25.0 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.875 J/g-°C
Thermal Conductivity 148 W/m-K
Melting Point 607 - 643 °C
Solidus 607 °C
Liquidus 643 °C
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 650 °F
Solution Temperature 750 °F
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 91 - 94.7 %As remainder
Chromium, Cr 0.06 - 0.20 %
Copper, Cu <= 0.10 %
Iron, Fe <= 0.40 %
Magnesium, Mg 1.0 - 1.8 %
Manganese, Mn 0.20 - 0.70 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si <= 0.35 %
Titanium, Ti 0.01 - 0.06 %
Zinc, Zn 4.0 - 5.0 %
Zirconium, Zr 0.08 - 0.20 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 7005-T6, 7005-T63, and 7005-T6351
Aluminum 7005-W
Aluminum 7005-O
Aluminum 7001-T75
Aluminum 7001-O

MA7005T53 / 9529

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.