MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Magnesium ZE41A-T5, Cast
Categories: Metal; Nonferrous Metal; Magnesium Alloy

Material Notes: Nd content refers to Nd-rich rare earths. Commercial and aerospace castings used in the artificially aged condition (T5 temper) with better castability than ZK51A and good strength up to 93°C. Useful in pressure tight applications.

Key Words: UNS M16410; Mg; AMS 4439; ASTM B 80; European EN 1753 MC35110 (Ingot UNS M16411)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.84 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 62500 kg load, 10 mm ball
Hardness, Knoop 83Estimated from Brinell
Hardness, Rockwell E 72
Hardness, Vickers 70Estimated from Brinell
Tensile Strength, Ultimate 205 MPa
Tensile Strength, Yield 140 MPa
@Strain 0.2 %
Elongation at Break 3.5 %in 50 mm
Tensile Modulus 45.0 GPa
Compressive Yield Strength 140 MPaat 0.2% offset
Compressive Strength 50000 psi
Ultimate Bearing Strength 485 MPa
Bearing Yield Strength 350 MPa
Poissons Ratio 0.35
Fatigue Strength 60.0 MPa
@# of Cycles 1.00e+7
Rotating Beam, R=-1, AZ910 Notched, Kt=2, Sand cast
 60.0 MPa
@# of Cycles 1.00e+7
Rotating Beam, R=-1 AZ910 Unnotched, Sand cast
 63.0 MPa
@# of Cycles 1.00e+6
Rotating Beam, R=-1, Unnotched, Sand cast
 65.0 MPa
@# of Cycles 1.00e+6
Rotating Beam, R=-1, AZ910 Notched, Kt=2, Sand cast
 85.0 MPa
@# of Cycles 1.00e+7
Rotating Beam, R=-1, ZE41A Notched, Kt=2, Sand cast
 90.0 MPa
@# of Cycles 1.00e+6
Rotating Beam, R=-1, ZE41A Notched, Kt=2, Sand cast
 96.0 MPa
@# of Cycles 100000
Rotating Beam, R=-1, AZ910 Unnotched, Sand cast
 98.0 MPa
@# of Cycles 1.00e+7
Rotating Beam, R=-1, ZE41A Unnotched, Sand cast
 98.0 MPa
@# of Cycles 100000
Rotating Beam, R=-1, AZ910 Notched, Kt=2, Sand cast
 101 MPa
@# of Cycles 1.00e+6
Rotating Beam, R=-1, ZE41A Unnotched, Sand cast
 110 MPa
@# of Cycles 100000
Rotating Beam, R=-1, ZE41A Notched, Kt=2, Sand cast
 130 MPa
@# of Cycles 100000
Rotating Beam, R=-1, ZE41A Unnotched, Sand cast
Machinability 100 %Relative Rating, 100=Best
Shear Modulus 17.0 GPa
Shear Strength 160 MPa
Charpy Impact 1.40 JV-notch
 1.40 JV-notch
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000600 ohm-cm
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 370 J/gEstimated from trends in similar Mg alloys.
CTE, linear 26.0 µm/m-°C
@Temperature 0.000 - 100 °C
Estimated from similar Mg alloys.
 27.0 µm/m-°C
@Temperature 20.0 - 200 °C
Estimated from similar Mg alloys
Specific Heat Capacity 1.00 J/g-°CTypical Mg alloy value.
Thermal Conductivity 113 W/m-K
Melting Point 525 - 645 °C
Solidus 525 °C
Liquidus 645 °C
 
Processing PropertiesOriginal ValueComments
Casting Temperature 750 - 820 °CSand Casting
 
Component Elements PropertiesOriginal ValueComments
Cerium, Ce 0.75 - 1.75 %
Copper, Cu <= 0.10 %
Magnesium, Mg 94 %
Manganese, Mn <= 0.15 %
Nickel, Ni <= 0.010 %
Zinc, Zn 3.5 - 5.0 %
Zirconium, Zr 0.40 - 1.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Magnesium ZK40A-T5, Extruded
Stratasys® Ultem 9085 for Rapid Prototyping
SEKISUI SPI KYDEX® 100 Polymer Alloy Sheet
Magnesium ZE63A-T6, Cast
AK Steel 17-4 PH® Precipitation Hardening Stainless Steel, Condition H 900

MMZE41 / 12472

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.