MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Plastcom SLOVALEN PQ 51 N Polypropylene Homopolymer, Modified with Elastomer, Impacted  (discontinued **)
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Impact Modified; Molded/Extruded

Material Notes: Features

Homopolymer PP modified with elastomer. The addition of thermoplastic elastomer causes increased toughness, possible alternative to PP copolymers. General application in all industry branches - packing material, garden flower-pots, toys, furniture industry, hinges, fasteners, clamps, office chairs, hangers etc. Delivered in natural and in the full RAL color scale.

Application: Injection Moulding

Information Provided by Plastcom spol. s r.o.

Key Words: PP
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.880 g/cc0.0318 lb/in³STN 64 0111
Linear Mold Shrinkage 0.018 cm/cm0.018 in/inSTN 64 0808
Linear Mold Shrinkage, Transverse 0.0183 cm/cm0.0183 in/inSTN 64 0808
Melt Flow 5.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
5.0 g/10 min
@Load 4.76 lb,
Temperature 446 °F
STN EN ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 30.0 MPa4350 psiSTN EN ISO 527-2
Elongation at Break 200 %200 %STN EN ISO 527-2
Tensile Modulus 1.10 GPa160 ksiSTN EN ISO 527-2
Flexural Strength 25.0 MPa3630 psiSTN EN ISO 178
Flexural Modulus 0.900 GPa131 ksiSTN EN ISO 178
Charpy Impact Unnotched  5.00 J/cm²
@Temperature -20.0 °C
23.8 ft-lb/in²
@Temperature -4.00 °F
STN EN ISO 179
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
STN EN ISO 179
Charpy Impact, Notched  0.200 J/cm²
@Temperature -20.0 °C
0.952 ft-lb/in²
@Temperature -4.00 °F
STN EN ISO 179
 0.500 J/cm²
@Temperature 23.0 °C
2.38 ft-lb/in²
@Temperature 73.4 °F
STN EN ISO 179
 
Thermal PropertiesMetricEnglishComments
Melting Point 140 °C284 °FDSC; STN EN ISO 3146
Deflection Temperature at 1.8 MPa (264 psi) 65.0 °C149 °FSTN EN ISO 75/A
Vicat Softening Point 125 °C257 °FB; STN EN ISO 306
 
Processing PropertiesMetricEnglishComments
Melt Temperature 200 - 250 °C392 - 482 °F
Mold Temperature 30.0 - 50.0 °C86.0 - 122 °F
Injection Pressure 60.0 - 70.0 MPa8700 - 10200 psi

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Arkema Pebax® 7233 SA 01 MED Polyether Block Amide (PEBA)
Arkema Pebax® 5533 SP 01 Polyether Block Amide (PEBA)
Arkema Pebax® 3533 SP 01 Polyether Block Amide (PEBA)
Flint Hills 44S2A Polypropylene Impact Copolymer
Ineos H20A-00 Polypropylene Homopolymer

PPLACO065 / 106943

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.