Physical Properties | Original Value | Comments |
---|
Density | 3.01 g/cc |
|
Chemical Properties | Original Value | Comments |
---|
Acid Class, SR | 52.3 |
Alkali Class, AR | 2.0 |
Stain Resistance Class, FR | 3.0 |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Knoop | 535 |
Modulus of Elasticity | 93.0 GPa |
Poissons Ratio | 0.249 |
Shear Modulus | 37.2 GPa |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear | 7.20 µm/m-°C @Temperature -30.0 - 70.0 °C |
| 8.90 µm/m-°C @Temperature 20.0 - 300 °C |
Specific Heat Capacity | 0.760 J/g-°C |
Thermal Conductivity | 1.01 W/m-K |
Transformation Temperature, Tg | 493 °C |
Softening Point | 593 °C |
Annealing Point | 494 °C |
|
Optical Properties | Original Value | Comments |
---|
Refractive Index | 1.555 @Wavelength 2323.4 nm |
| 1.561 @Wavelength 1970.1 nm |
| 1.567 @Wavelength 1529.6 nm |
| 1.574 @Wavelength 1014 nm |
| 1.574 @Wavelength 1060 nm |
| 1.577 @Wavelength 852.1 nm |
| 1.581 @Wavelength 706.5 nm |
| 1.582 @Wavelength 656.3 nm |
| 1.583 @Wavelength 632.8 nm |
| 1.583 @Wavelength 643.8 nm |
| 1.585 @Wavelength 589.3 nm |
| 1.586 @Wavelength 587.6 nm |
| 1.588 @Wavelength 546.1 nm |
| 1.592 @Wavelength 486.1 nm |
| 1.593 @Wavelength 480 nm |
| 1.598 @Wavelength 435.8 nm |
| 1.602 @Wavelength 404.7 nm |
| 1.61 @Wavelength 365 nm |
| 1.618 @Wavelength 334.1 nm |
Abbe Number | 59.26 |
| 59.5 |
Optical Dispersion | 0.009849 |
| 0.009928 |
Transmission, Visible | 98.7 % @Thickness 25.0 mm, Wavelength 420 nm |
| 98.9 % @Thickness 25.0 mm, Wavelength 436 nm |
| 99.1 % @Thickness 25.0 mm, Wavelength 460 nm |
| 99.5 % @Thickness 10.0 mm, Wavelength 420 nm |
| 99.5 % @Thickness 25.0 mm, Wavelength 500 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 436 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 460 nm |
| 99.7 % @Thickness 25.0 mm, Wavelength 620 nm |
| 99.7 % @Thickness 25.0 mm, Wavelength 546 nm |
| 99.7 % @Thickness 25.0 mm, Wavelength 660 nm |
| 99.7 % @Thickness 25.0 mm, Wavelength 700 nm |
| 99.7 % @Thickness 25.0 mm, Wavelength 580 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 500 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 546 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 700 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 660 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 580 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 620 nm |
IR Transmittance | 40 % @Thickness 25.0 mm, Wavelength 2500 nm |
| 63 % @Thickness 25.0 mm, Wavelength 2325 nm |
| 69.3 % @Thickness 10.0 mm, Wavelength 2500 nm |
| 83.1 % @Thickness 10.0 mm, Wavelength 2325 nm |
| 89 % @Thickness 25.0 mm, Wavelength 1970 nm |
| 95.4 % @Thickness 10.0 mm, Wavelength 1970 nm |
| 97.8 % @Thickness 25.0 mm, Wavelength 1530 nm |
| 99.1 % @Thickness 10.0 mm, Wavelength 1530 nm |
| 99.7 % @Thickness 25.0 mm, Wavelength 1060 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 1060 nm |
UV Transmittance | 12.3 % @Thickness 10.0 mm, Wavelength 310 nm |
| 16 % @Thickness 25.0 mm, Wavelength 320 nm |
| 48 % @Thickness 10.0 mm, Wavelength 320 nm |
| 61 % @Thickness 25.0 mm, Wavelength 334 nm |
| 82.1 % @Thickness 10.0 mm, Wavelength 334 nm |
| 87 % @Thickness 25.0 mm, Wavelength 350 nm |
| 94.6 % @Thickness 10.0 mm, Wavelength 350 nm |
| 95 % @Thickness 25.0 mm, Wavelength 365 nm |
| 96 % @Thickness 25.0 mm, Wavelength 370 nm |
| 97.3 % @Thickness 25.0 mm, Wavelength 380 nm |
| 98 % @Thickness 25.0 mm, Wavelength 390 nm |
| 98 % @Thickness 10.0 mm, Wavelength 365 nm |
| 98.4 % @Thickness 10.0 mm, Wavelength 370 nm |
| 98.4 % @Thickness 25.0 mm, Wavelength 400 nm |
| 98.5 % @Thickness 25.0 mm, Wavelength 405 nm |
| 98.9 % @Thickness 10.0 mm, Wavelength 380 nm |
| 99.2 % @Thickness 10.0 mm, Wavelength 390 nm |
| 99.4 % @Thickness 10.0 mm, Wavelength 400 nm |
| 99.4 % @Thickness 10.0 mm, Wavelength 405 nm |
|
Descriptive Properties |
---|
Acid resistance class | 4 |
Climatic resistance | 4 |
Grindability | 124 |
| 3 |
Phosphate resistance | 3 |
Stress optical coefficient | 2.17 |
Water resistance class | 1 |
Yield point/sag temperature | 522°C |