MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Morgan Advanced Ceramics Kaolite® 2200 Gun Thermal Ceramic
Categories: Ceramic; Oxide

Material Notes: Crystalline Silica. Gun installation. Kaolite 2200 Gun is designed for temperatures up to 2200°F (1204°C). It has excellent volume stability and good strength. This general purpose, lightweight monolithics have low density, excellent resistance to thermal shock, and low thermal conductivity.

Applications:

  • Backup insulation in two component linings in petrochemical process units
  • Hot face lining in ductwork from waste heat recovery boilers and process unit
  • F.C.C.U. linings-regenerator
  • Hydrogen or reducing atmosphere linings
  • Radiant section in steam flood generators
  • Hydrogen or reducing atmosphere linings
  • Steam flood generator convection sections and target walls.

Information provided by Morgan Advanced Materials

Key Words: Thermal Ceramics
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.897 - 1.073 g/cc
@Temperature 816 °C
0.0324 - 0.03876 lb/in³
@Temperature 1500 °F
fired; ASTM C 134
 1.009 - 1.186 g/cc
@Temperature 104 °C,
Time 86400 sec
0.03645 - 0.04285 lb/in³
@Temperature 219 °F,
Time 24.0 hour
dried; ASTM C 134
 
Mechanical PropertiesMetricEnglishComments
Modulus of Rupture  0.000620 - 0.00103 GPa
@Temperature 104 °C,
Time 86400 sec
0.0899 - 0.149 ksi
@Temperature 219 °F,
Time 24.0 hour
dried; ASTM C133
 0.000760 - 0.00155 GPa
@Temperature 816 °C,
Time 18000 sec
0.110 - 0.225 ksi
@Temperature 1500 °F,
Time 5.00 hour
fired; ASTM C133
 0.000900 - 0.00172 GPa
@Temperature 1204 °C,
Time 18000 sec
0.131 - 0.249 ksi
@Temperature 2199 °F,
Time 5.00 hour
fired; ASTM C133
Compressive Strength  2.06 - 3.50 MPa
@Temperature 104 °C,
Time 86400 sec
299 - 508 psi
@Temperature 219 °F,
Time 24.0 hour
Cold Crushing Strength, dried; ASTM C133
 2.76 - 6.20 MPa
@Temperature 816 °C,
Time 18000 sec
400 - 899 psi
@Temperature 1500 °F,
Time 5.00 hour
Cold Crushing Strength, fired; ASTM C133
 3.10 - 62.0 MPa
@Temperature 1204 °C,
Time 18000 sec
450 - 8990 psi
@Temperature 2199 °F,
Time 5.00 hour
Cold Crushing Strength, fired; ASTM C133
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity  0.210 W/m-K
@Temperature 260 °C
1.46 BTU-in/hr-ft²-°F
@Temperature 500 °F
ASTM C201
 0.230 W/m-K
@Temperature 538 °C
1.60 BTU-in/hr-ft²-°F
@Temperature 1000 °F
ASTM C201
 0.260 W/m-K
@Temperature 815 °C
1.80 BTU-in/hr-ft²-°F
@Temperature 1500 °F
ASTM C201
 0.280 W/m-K
@Temperature 1093 °C
1.94 BTU-in/hr-ft²-°F
@Temperature 1999 °F
ASTM C201
Maximum Service Temperature, Air <= 1204 °C<= 2199 °F
Shrinkage  0.00 - 0.20 %
@Treatment Temp. 104 °C,
Time 86400 sec
0.00 - 0.20 %
@Treatment Temp. 219 °F,
Time 24.0 hour
dried
 0.20 - 0.65 %
@Treatment Temp. 816 °C,
Time 18000 sec
0.20 - 0.65 %
@Treatment Temp. 1500 °F,
Time 5.00 hour
fired
 0.30 - 0.80 %
@Treatment Temp. 1204 °C,
Time 18000 sec
0.30 - 0.80 %
@Treatment Temp. 2199 °F,
Time 5.00 hour
fired
 
Processing PropertiesMetricEnglishComments
Shelf Life 12.0 Month12.0 Month
 
Component Elements PropertiesMetricEnglishComments
Al2O3 36 %36 %
CaO 17 %17 %
Fe2O3 1.6 %1.6 %
K2O+Na2O 1.4 %1.4 %Na2O & K2O
MgO 0.20 %0.20 %
SiO2 42 %42 %
TiO2 1.4 %1.4 %
 
Descriptive Properties
Placement, average (kg)993to place 1m3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

CMORF6351 / 203135

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.