MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
LATI LASTIROL TR G/10-V1 10% Glass Fiber Reinforced Polystyrene (PS) (UL94 V-1)  (discontinued **)
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Glass Filled

Material Notes: Description: Lastirol thermoplastics are polystyrene (PS) products. The Lastirols feature excellent dimensional stability, good flowability, and can be molded without any particular problem. Glass fiber reinforced types have high rigidity and excellent dimensional stability.

Specific Notes for this Material: UL94V-1 self-extinguishing, with halogens; 10% glass fiber; good dimensional stability.

Disclaimer from LATI: This document contains information based on average values as obtained from the results of laboratory tests and observations made on LATI materials. Tested materials were injection molded, used in their natural color, and conditioned in compliance with Standard ASTM D 618, procedure A. These values refer to LATI's best technical and scientific knowledge at the moment of testing and cannot be used as a basis for the development of applications. For a better assessment of the materials, you are kindly requested to contact LATI's technical or commercial offices, which are at your disposal and will supply detailed information on the most suitable characteristics for their intended use. With reference to DPR n.224 dated May 24, 1988, issued in accordance with EC Guide-lines 85/374, LATI Industria Termoplastici S.p.A. declines all responsibility arising from an improper use of the products described in this document.

All data provided by LATI.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.20 g/ccISO 1183
Water Absorption 0.060 %at 23°C; ISO 62
Linear Mold Shrinkage 0.0025 cm/cmLATI
Linear Mold Shrinkage, Transverse 0.0025 cm/cmLATI
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 50ASTM D785
Tensile Strength, Ultimate 40.0 MPaISO 527
 25.0 MPa
@Temperature 60.0 °C
ISO 527
Flexural Modulus 3.50 GPaASTM D790
 3.30 GPa
@Temperature 60.0 °C
ASTM D790
Izod Impact, Notched 0.400 J/cm
@Temperature -40.0 °C
ASTM D256
 45.0 J/m
@Temperature -20.0 °C
ASTM D256
 75.0 J/m
@Temperature 23.0 °C
ASTM D256
Charpy Impact Unnotched 2.00 J/cm²
@Temperature -20.0 °C
DIN 53453
 2.00 J/cm²
@Temperature -40.0 °C
DIN 53453
 2.00 J/cm²
@Temperature 23.0 °C
DIN 53453
 
Electrical PropertiesOriginal ValueComments
Dielectric Strength 23.0 kV/mm
@Thickness 2.00 mm
IEC 243-1
Comparative Tracking Index 375 VIEC 112
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 92.0 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 81.0 °CASTM D648
Vicat Softening Point 95.0 °C50°C/h 50N; ISO 306
Flammability, UL94 V-2
@Thickness 1.50 mm
 V-1
@Thickness 3.00 mm
Oxygen Index 24 %ISO 4589
Glow Wire Test 960 °C
@Thickness 2.00 mm
IEC 695-2-1
 960 °C
@Thickness 1.00 mm
IEC 695-2-1
 
Processing PropertiesOriginal ValueComments
Melt Temperature 180 - 200 °C
Mold Temperature 30.0 - 50.0 °C
Drying Temperature 60.0 - 70.0 °CTemperature can be reduced when using vacuum ovens.
Dry Time >= 3 hourDrying time can be reduced when using vacuum ovens.
 
Descriptive Properties
Heat Resistance - Ball Test (125°C)NIEC 335
Heat Resistance - Ball Test (165°C)NIEC 335
Injection Speedmedium
Needle Burner TestY1.47 mm
 Y3.05 mm

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
A. Schulman ComAlloy Hiloy® 213 Polystyrene, Glass Reinforced
Overview of materials for Polystyrene, Glass Filled
Overview of materials for Polystyrene, Transparent Grade
RTP Company RTP 406  Polystyrene (PS) Glass Fiber 35%
RTP Company RTP 401 Polystyrene (PS), Glass Fiber

PLATI159 / 50157

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.