MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
SABIC LNP™ THERMOCOMP™ Compound RF0029S Polyamide 66 (Nylon 66)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66)

Material Notes: LNP THERMOCOMP RF0029S compound is based on Nylon 6/6 resin containing 10% glass fiber. Added features of this grade include: Flame Retardant, Heat Stabilized.

Features: High Stiffness,Flame Retardant,Heat Stabilized,Structural

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.48 g/ccASTM D792
 1.48 g/ccISO 1183
Moisture Absorption 0.150 - 0.250 %Injection Molding
 0.500 %23°C/50% RH/24 hrs; ASTM D570
Linear Mold Shrinkage, Flow 0.0098 cm/cm24hrs; ISO 294
 0.0090 - 0.011 cm/cm24hrs; ASTM D955
Linear Mold Shrinkage, Transverse 0.012 - 0.014 cm/cm24hrs; ASTM D955
 0.013 cm/cm24hrs; ISO 294
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 101 MPaASTM D638
 102 MPaISO 527
Tensile Strength, Yield 101 MPaASTM D638
 102 MPaISO 527
Elongation at Break 2.4 %ISO 527
 2.5 %ASTM D638
Elongation at Yield 2.4 %ISO 527
 2.5 %ASTM D638
Tensile Modulus 6370 MPa1 mm/min; ISO 527
 6890 MPa50 mm/min; ASTM D638
Flexural Strength 150 MPaISO 178
 151 MPaASTM D790
Flexural Modulus 5510 MPaASTM D790
 5900 MPaISO 178
Izod Impact Notched 42.0 JASTM D256
Izod Impact, Unnotched 501 J/mASTM D4812
Izod Impact, Notched (ISO) 5.00 kJ/m²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 33.0 kJ/m²80*10*4; ISO 180/1U
Dart Drop, Total Energy 8.00 Jpeak; ASTM D3763
Impact Test 1.00 JMultiaxial Impact; ISO 6603
 
Electrical PropertiesOriginal ValueComments
Arc Resistance 0.00 - 60 secASTM D495
Comparative Tracking Index 175 - 250 VUL 746A
Hot Wire Ignition, HWI 60 - 120 sec
@Thickness >=1.70 mm
UL 746A
 >= 120 sec
@Thickness >=3.00 mm
UL 746A
High Amp Arc Ignition, HAI 60 - 120 arcs
@Thickness >=1.70 mm
UL 746A
 >= 120 arcs
@Thickness >=3.00 mm
UL 746A
High Voltage Arc-Tracking Rate, HVTR 10.0 - 25.4 mm/minUL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 42.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
 43.2 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
CTE, linear, Transverse to Flow 75.6 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 76.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 249 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 252 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 219 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 233 °C
@Thickness 3.20 mm
unannealed; ASTM D648
UL RTI, Electrical 130 °CUL 746B
UL RTI, Mechanical with Impact 105 °CUL 746B
UL RTI, Mechanical without Impact 115 °CUL 746B
Flammability, UL94 V-0
@Thickness >=1.70 mm
UL 94
 
Processing PropertiesOriginal ValueComments
Zone 2 280 - 295 °C
Zone 3 295 - 305 °C
Melt Temperature 275 - 290 °CInjection Molding
Mold Temperature 80.0 - 95.0 °C
Drying Temperature 80.0 °CInjection Molding
Dry Time 4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa
Screw Speed 30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH81838 / 289785

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.