MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Envalior Durethan® B 30 S F30 000000 Nylon 6 (PA6), Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Unreinforced

Material Notes: PA 6, non-reinforced, injection molding, flame retardant

Former Lanxess product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.35 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.011 cm/cm60x60x2; 260 °C / MT 80°C; 600 bar; ISO 294-4
Linear Mold Shrinkage, Transverse 0.011 cm/cm60x60x2; 260 °C / MT 80°C; 600 bar; ISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 70.0 MPa50 mm/min; ISO 527-1,-2
Elongation at Break 9.0 %50 mm/min, Nominal; ISO 527-1,-2
Elongation at Yield 3.7 %50 mm/min; ISO 527-1,-2
Tensile Modulus 3600 MPa1 mm/min; ISO 527-1,-2
Flexural Strength 110 MPa2 mm/min; ISO 178-A
Flexural Yield Strength 100 MPa
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Modulus 3200 MPa2 mm/min; ISO 178-A
Flexural Strain at Break 5.5 %2 mm/min; ISO 178-A
Izod Impact, Notched (ISO) <= 10.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1A
 <= 10.0 kJ/m²
@Temperature -30.0 °C
ISO 180-1A
Izod Impact, Unnotched (ISO) 100 kJ/m²
@Temperature -30.0 °C
ISO 180-1U
 120 kJ/m²
@Temperature 23.0 °C
ISO 180-1U
Charpy Impact Unnotched 130 kJ/m²
@Temperature -30.0 °C
ISO 179-1eU
 150 kJ/m²
@Temperature 23.0 °C
ISO 179-1eU
Charpy Impact, Notched <= 10.0 kJ/m²
@Temperature 23.0 °C
ISO 179 1eA
 <= 10.0 kJ/m²
@Temperature -30.0 °C
ISO 179 1eA
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 300 VSolution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
Melting Point 222 °C10°C/min; ISO 11357-1,-3
Flammability, UL94 V-0
@Thickness 0.400 mm
 V-0
@Thickness 0.750 mm
 V-0
@Thickness 1.50 mm
 5VA
@Thickness 2.00 mm
 5VA
@Thickness 3.00 mm
Glow Wire Ignition Temperature 800 °C
@Thickness 3.00 mm
IEC 60695-2-13
 825 °C
@Thickness 0.750 mm
IEC 60695-2-13
 825 °C
@Thickness 1.50 mm
IEC 60695-2-13
Glow Wire Flammability Index 960 °C
@Thickness 0.800 mm
IEC 60695-2-12
 960 °C
@Thickness 1.50 mm
IEC 60695-2-12
 960 °C
@Thickness 3.00 mm
IEC 60695-2-12
Shrinkage, MD 0.40 %
@Treatment Temp. 120 °C,
Time 14400 sec
Flow Direction Post-Molding, 60x60x2; ISO 294-4
Shrinkage, TD 0.40 %
@Treatment Temp. 120 °C,
Time 14400 sec
Post-Molding, 60x60x2; ISO 294-4
 
Processing PropertiesOriginal ValueComments
Melt Temperature 260 °Cinjection molding; ISO 294
 250 - 270 °C
Mold Temperature 80.0 °Cinjection molding; ISO 294
 80.0 - 100 °C
Drying Temperature 80.0 °C
Dry Time 2.00 - 6.00 hour
Moisture Content 0.030 - 0.12 %Karl Fischer

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Avient Bergamid™ B700 UF black Polyamide 6 (Nylon 6), DAM
Envalior Durethan® B 30 S FN30 000000 Nylon 6 (PA6), Dry
Celanese Nilit FRIANYL B63 HS-GV10 Nylon 6 for injection molding, 10% glass fiber reinforced
Domo TECHNYL® C 50 H2 PA6, DRY
Covestro Bayblend® FR3000 PC/ABS Blend

PLANW9258 / 208059

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.