MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Overview of materials for Cellulose Acetate Propionate, Molded
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Cellulosic; Cellulose Acetate Propionate, Molded

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Cellulose Acetate Propionate, Molded". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.17 - 1.21 g/ccAverage value: 1.20 g/cc Grade Count:79
Water Absorption 1.30 - 1.80 %Average value: 1.51 % Grade Count:70
Linear Mold Shrinkage 0.00200 - 0.00600 cm/cmAverage value: 0.00400 cm/cm Grade Count:78
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 40.0 - 95.0Average value: 75.5 Grade Count:38
Tensile Strength, Ultimate 23.0 - 41.4 MPaAverage value: 33.3 MPa Grade Count:72
 8.00 - 8.00 MPa
@Temperature 120 - 120 °C
Average value: 8.00 MPa Grade Count:1
Tensile Strength, Yield 19.4 - 41.4 MPaAverage value: 30.1 MPa Grade Count:79
Elongation at Break 34.0 - 86.0 %Average value: 42.7 % Grade Count:58
Elongation at Yield 3.00 - 25.0 %Average value: 5.95 % Grade Count:10
 160 - 160 %
@Temperature 120 - 120 °C
Average value: 160 % Grade Count:1
Modulus of Elasticity 0.927 - 1.85 GPaAverage value: 1.52 GPa Grade Count:10
 1.40 - 1.40 GPa
@Temperature 120 - 120 °C
Average value: 1.40 GPa Grade Count:1
Flexural Yield Strength 29.0 - 55.8 MPaAverage value: 39.5 MPa Grade Count:70
Flexural Modulus 0.981 - 1.86 GPaAverage value: 1.38 GPa Grade Count:65
Izod Impact, Notched 1.76 - 5.33 J/cmAverage value: 3.88 J/cm Grade Count:71
 0.750 - 1.23 J/cm
@Temperature -40.0 - -40.0 °C
Average value: 1.02 J/cm Grade Count:50
Charpy Impact Unnotched NBGrade Count:8
 NB - NB
@Temperature -30.0 - -30.0 °C
Grade Count:8
Charpy Impact, Notched 0.580 - 2.61 J/cm²Average value: 1.72 J/cm² Grade Count:8
 0.340 - 1.05 J/cm²
@Temperature -30.0 - -30.0 °C
Average value: 0.707 J/cm² Grade Count:8
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1.00e+13 - 1.00e+15 ohm-cmAverage value: 5.05e+14 ohm-cm Grade Count:48
Dielectric Constant 3.30 - 3.80Average value: 3.55 Grade Count:48
Dielectric Strength 11.8 - 18.7 kV/mmAverage value: 15.3 kV/mm Grade Count:41
Dissipation Factor 0.0100 - 0.150Average value: 0.0800 Grade Count:48
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.0 - 170 µm/m-°CAverage value: 86.5 µm/m-°C Grade Count:56
CTE, linear, Transverse to Flow 122 - 140 µm/m-°CAverage value: 132 µm/m-°C Grade Count:8
Specific Heat Capacity 1.26 - 1.67 J/g-°CAverage value: 1.46 J/g-°C Grade Count:48
Thermal Conductivity 0.170 - 0.330 W/m-KAverage value: 0.248 W/m-K Grade Count:48
Deflection Temperature at 0.46 MPa (66 psi) 65.0 - 96.0 °CAverage value: 84.4 °C Grade Count:58
Deflection Temperature at 1.8 MPa (264 psi) 64.0 - 101 °CAverage value: 76.1 °C Grade Count:79
Vicat Softening Point 81.0 - 107 °CAverage value: 95.8 °C Grade Count:79
Glass Transition Temp, Tg 90.0 - 111 °CAverage value: 103 °C Grade Count:9
Flammability, UL94 HBGrade Count:3
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.46 - 1.49Average value: 1.47 Grade Count:50
Haze 8.50 %Average value: 8.50 % Grade Count:49
Transmission, Visible 71.0 - 90.0 %Average value: 89.7 % Grade Count:50
 
Processing PropertiesOriginal ValueComments
Melt Temperature 207 - 250 °CAverage value: 227 °C Grade Count:29
Mold Temperature 43.0 - 74.0 °CAverage value: 56.0 °C Grade Count:21

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Cellulose Acetate, Molded
Overview of materials for Cellulose Acetate Butyrate, Molded
304 Stainless Steel
Eastman Tenite Propionate 376E4000012 Clear, Trsp Cellulose Acetate Propionate
Overview of materials for Ethyl Cellulose, Molded

O1650 / 77884

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.