MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
ExxonMobil Exxtra™ Seal POP 4573 Plastomer for Elastic Film and Elastic Film Blends
Categories: Polymer; Film; Thermoplastic; Elastomer, TPE

Material Notes: Product Description: Exxtra™ Seal POP 4573 is an ethylene-based butene plastomer produced using ExxonMobil Chemical's EXXPOL® Catalyst Technology. This resin is designed for use as the cling component in multilayer stretch film and surface protective films. Seal POP 4573 can also be used in multilayer castfilm applications requiring high tensile extension and good elastic recovery/snap back

Availability: Latin America, North America

Additive:

  • Antiblock: No
  • Slip: No
  • Thermal Stabilizer: Yes
Applications:
  • Cling Layer
Information provided by ExxonMobil Chemical

Key Words: EXACT™ 4049
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.873 g/ccExxonMobil Method
Melt Flow 4.5 g/10 min190°C/2.16kg; ExxonMobil Method
 
Thermal PropertiesOriginal ValueComments
Melting Point 132 °FPeak Melting Temperature; ExxonMobil Method
Crystallization Temperature 41.0 °CExxonMobil Method
Vicat Softening Point 131 °FASTM D1525
 
Descriptive Properties
FeaturesThermal Stabilizer

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Sika AcouBond®-System Elastic Bonding and Acoustical Dampening
ExxonMobil Santoprene® 521-70 Thermoplastic Rubber
Armacell OleTex® BDJN 200 EVA/LDPE Foam
3D Systems FabPro™ Elastic BLK Elastomer
Dow AFFINITY™ KC 8852 Polyolefin Elastomer

PEXB351 / 37656

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.