MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ohara S-LAH99 Optical Glass
Categories: Ceramic; Glass; Optical

Material Notes: This material can be used for a variety of uses such as interchangeable photographic lenses, projectors, and various other applications. S-LAH99 is an effective option for both cost reduction and higher performance.

Information provided by Ohara Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 5.02 g/cc5.02 g/cc
 
Chemical PropertiesMetricEnglishComments
Acid Class, SR 2.02.0
 
Mechanical PropertiesMetricEnglishComments
Hardness, Knoop 650
@Load 0.0999 kg
650
@Load 0.220 lb
Modulus of Elasticity 131.3 GPa19040 ksi
Modulus of Rigidity 50.2 GPa7280 ksi
Poissons Ratio 0.3070.307
Abrasion 5555Aa
 
Thermal PropertiesMetricEnglishComments
CTE, linear  7.50 µm/m-°C
@Temperature -30.0 - 70.0 °C
4.17 µin/in-°F
@Temperature -22.0 - 158 °F
 8.80 µm/m-°C
@Temperature 100 - 300 °C
4.89 µin/in-°F
@Temperature 212 - 572 °F
Thermal Conductivity 0.944 W/m-K
@Temperature 35.0 °C
6.55 BTU-in/hr-ft²-°F
@Temperature 95.0 °F
Transformation Temperature, Tg 725 °C1340 °Fper thermal expansion curve
Softening Point 792 °C1460 °F107.65 poise; JIS-R3104 and ASTM-C338
Annealing Point 718 °C1320 °F1013 poise; ASTM-C336
Strain Point 682 °C1260 °F1014.5 poise; JIS-R3103 and ASTM-C336
 
Optical PropertiesMetricEnglishComments
Refractive Index  1.93863
@Wavelength 2325.42 nm
1.93863
@Wavelength 2325.42 nm
 1.94585
@Wavelength 1970.09 nm
1.94585
@Wavelength 1970.09 nm
 1.9544
@Wavelength 1529.58 nm
1.9544
@Wavelength 1529.58 nm
 1.9638
@Wavelength 1128.64 nm
1.9638
@Wavelength 1128.64 nm
 1.96756
@Wavelength 1013.98 nm
1.96756
@Wavelength 1013.98 nm
nt (Hg t line)
 1.97488
@Wavelength 852.11 nm
1.97488
@Wavelength 852.11 nm
ns (Cs s line)
 1.98035
@Wavelength 768.19 nm
1.98035
@Wavelength 768.19 nm
nA' (K A' line)
 1.98561
@Wavelength 706.52 nm
1.98561
@Wavelength 706.52 nm
nr (He r line)
 1.99105
@Wavelength 656.27 nm
1.99105
@Wavelength 656.27 nm
nC (H C line)
 1.9926
@Wavelength 643.85 nm
1.9926
@Wavelength 643.85 nm
nC' (Cd C' line)
 1.99406
@Wavelength 632.8 nm
1.99406
@Wavelength 632.8 nm
nHe-Ne
 2.0007
@Wavelength 589.29 nm
2.0007
@Wavelength 589.29 nm
nD
 2.001
@Wavelength 587.56 nm
2.001
@Wavelength 587.56 nm
nd (He D line)
 2.00912
@Wavelength 546.07 nm
2.00912
@Wavelength 546.07 nm
ne (Hg e line)
 2.0254
@Wavelength 486.13 nm
2.0254
@Wavelength 486.13 nm
nf (H F line)
 2.02749
@Wavelength 479.99 nm
2.02749
@Wavelength 479.99 nm
nF' (Cd F' line)
 2.04319
@Wavelength 441.57 nm
2.04319
@Wavelength 441.57 nm
nHe-Cd
 2.046
@Wavelength 435.835 nm
2.046
@Wavelength 435.835 nm
ng (Hg g line)
 2.06424
@Wavelength 404.656 nm
2.06424
@Wavelength 404.656 nm
nh (Hg h line)
Abbe Number 28.9228.92ν e
 29.1429.14ν d
Optical Dispersion 0.0099520.009952nd-nC; Partial Dispersion
 0.0106950.010695nC-nA'; Partial Dispersion
 0.0165190.016519ne-nC'; Partial Dispersion
 0.018070.01807ne-nC; Partial Dispersion
 0.0182350.018235nh-ng; Partial Dispersion
 0.0183760.018376nF'-ne; Partial Dispersion
 0.0206010.020601ng-nF; Partial Dispersion
 0.023490.02349nC-nt; Partial Dispersion
 0.0250410.025041nC'-nt; Partial Dispersion
 0.0343520.034352nF-nC
 0.0348950.034895nF'-nC'
 0.0450010.045001ng-nd; Partial Dispersion
Transmission, Visible  49 %
@Thickness 10.0 mm,
Wavelength 380 nm
49 %
@Thickness 0.394 in,
Wavelength 380 nm
Internal Transmission
 66 %
@Thickness 10.0 mm,
Wavelength 390 nm
66 %
@Thickness 0.394 in,
Wavelength 390 nm
Internal Transmission
 76 %
@Thickness 10.0 mm,
Wavelength 400 nm
76 %
@Thickness 0.394 in,
Wavelength 400 nm
Internal Transmission
 87 %
@Thickness 10.0 mm,
Wavelength 420 nm
87 %
@Thickness 0.394 in,
Wavelength 420 nm
Internal Transmission
 92.4 %
@Thickness 10.0 mm,
Wavelength 440 nm
92.4 %
@Thickness 0.394 in,
Wavelength 440 nm
Internal Transmission
 95.1 %
@Thickness 10.0 mm,
Wavelength 460 nm
95.1 %
@Thickness 0.394 in,
Wavelength 460 nm
Internal Transmission
 96.8 %
@Thickness 10.0 mm,
Wavelength 480 nm
96.8 %
@Thickness 0.394 in,
Wavelength 480 nm
Internal Transmission
 98 %
@Thickness 10.0 mm,
Wavelength 500 nm
98 %
@Thickness 0.394 in,
Wavelength 500 nm
Internal Transmission
 99.5 %
@Thickness 10.0 mm,
Wavelength 550 nm
99.5 %
@Thickness 0.394 in,
Wavelength 550 nm
Internal Transmission
 99.8 %
@Thickness 10.0 mm,
Wavelength 600 nm
99.8 %
@Thickness 0.394 in,
Wavelength 600 nm
Internal Transmission
 99.8 %
@Thickness 10.0 mm,
Wavelength 650 nm
99.8 %
@Thickness 0.394 in,
Wavelength 650 nm
Internal Transmission
 99.9 %
@Thickness 10.0 mm,
Wavelength 700 nm
99.9 %
@Thickness 0.394 in,
Wavelength 700 nm
Internal Transmission
IR Transmittance  88 %
@Thickness 10.0 mm,
Wavelength 2400 nm
88 %
@Thickness 0.394 in,
Wavelength 2400 nm
Internal Transmission
 96.4 %
@Thickness 10.0 mm,
Wavelength 2200 nm
96.4 %
@Thickness 0.394 in,
Wavelength 2200 nm
Internal Transmission
 98.3 %
@Thickness 10.0 mm,
Wavelength 2000 nm
98.3 %
@Thickness 0.394 in,
Wavelength 2000 nm
Internal Transmission
 99.5 %
@Thickness 10.0 mm,
Wavelength 1800 nm
99.5 %
@Thickness 0.394 in,
Wavelength 1800 nm
Internal Transmission
 99.8 %
@Thickness 10.0 mm,
Wavelength 1600 nm
99.8 %
@Thickness 0.394 in,
Wavelength 1600 nm
Internal Transmission
 99.9 %
@Thickness 10.0 mm,
Wavelength 800 nm
99.9 %
@Thickness 0.394 in,
Wavelength 800 nm
Internal Transmission
 99.9 %
@Thickness 10.0 mm,
Wavelength 900 nm
99.9 %
@Thickness 0.394 in,
Wavelength 900 nm
Internal Transmission
 99.9 %
@Thickness 10.0 mm,
Wavelength 1000 nm
99.9 %
@Thickness 0.394 in,
Wavelength 1000 nm
Internal Transmission
 99.9 %
@Thickness 10.0 mm,
Wavelength 1200 nm
99.9 %
@Thickness 0.394 in,
Wavelength 1200 nm
Internal Transmission
 99.9 %
@Thickness 10.0 mm,
Wavelength 1400 nm
99.9 %
@Thickness 0.394 in,
Wavelength 1400 nm
Internal Transmission
UV Transmittance  5.0 %
@Thickness 10.0 mm,
Wavelength 360 nm
5.0 %
@Thickness 0.394 in,
Wavelength 360 nm
Internal Transmission
 25 %
@Thickness 10.0 mm,
Wavelength 370 nm
25 %
@Thickness 0.394 in,
Wavelength 370 nm
Internal Transmission
 
Descriptive Properties
Acid Resistance, Powder Method, RA(P)1
CCI0.00 B
 5 G
 5 R
coloring, λ 5360
coloring, λ 70425
Coloring, Internal Transmission λ 0.05360
Coloring, Internal Transmission λ 0.80407
Knoop Hardness Class7
Ohara Code d001291
Ohara Code e009289
Phosphate Resistance, PR1
Photoelastic Constant (ß)0.76
Water Resistance, RW(P)1
Weathering Resistance (Surface Method) W(S)max1
Yield Point, At (°C)761per thermal expansion curve

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

CZOHARA771 / 281610

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.