MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Envalior Durethan® BM 40 X H2.0 DUS009 901510 Nylon 6 (PA6), 40% Glass/Mineral Reinforced, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Glass/Mineral Reinforced

Material Notes: PA 6, injection molding grade, 40% glass fibers/mineral, good heat-ageing resistance

Former Lanxess product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.48 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.0043 cm/cm150x105x3; ISO 2577
 0.0051 cm/cm60x60x2; ISO 2577
Linear Mold Shrinkage, Transverse 0.0067 cm/cm60x60x2; ISO 2577
 0.0108 cm/cm150x105x3; ISO 2577
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 213 MPaISO 2093-1
Tensile Strength at Break 120 MPa5 mm/min; ISO 527-1,-2
Elongation at Break 2.8 %5 mm/min; ISO 527-1,-2
Tensile Modulus 8000 MPa1 mm/min; ISO 527-1,-2
Flexural Strength 193 MPa2 mm/min; ISO 178-A
Flexural Yield Strength 193 MPa
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Modulus 7500 MPa2 mm/min; ISO 178-A
Flexural Strain at Break 3.6 %2 mm/min; ISO 178-A
Izod Impact, Notched (ISO) <= 10.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1A
Izod Impact, Unnotched (ISO) 35.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1U
 35.0 kJ/m²
@Temperature -30.0 °C
ISO 180-1U
Charpy Impact Unnotched 40.0 kJ/m²
@Temperature -30.0 °C
ISO 180-1U
 45.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1U
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 425 VSolution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 40.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
CTE, linear, Transverse to Flow 80.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
Melting Point 221 °C10°C/min; ISO 11357-1,-3
Deflection Temperature at 0.46 MPa (66 psi) 190 °CISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 215 °CISO 75-1,-2
Deflection Temperature at 8.0 MPa 80.0 °CISO 75-1,-2
Vicat Softening Point 215 °C
@Load 5.10 kg
120°C/h; ISO 306
Flammability, UL94 HB
@Thickness 0.750 mm
Shrinkage, MD 0.060 %
@Treatment Temp. 120 °C,
Time 14400 sec
Post-Shrinkage Flow Direction 150x105x3; ISO 2577
 0.17 %
@Treatment Temp. 120 °C,
Time 14400 sec
Post-Shrinkage Flow Direction; 60x60x2; ISO 2577
Shrinkage, TD 0.060 %
@Treatment Temp. 120 °C,
Time 14400 sec
150x105x3; ISO 2577
 0.15 %
@Treatment Temp. 120 °C,
Time 14400 sec
60x60x2; ISO 2577
 
Processing PropertiesOriginal ValueComments
Melt Temperature 290 °C
Mold Temperature 80.0 °C
Back Pressure 50.0 - 60.0 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Eurotec® Tecomid® NB40 KK40 NL PA6, 40% glass fiber/mineral reinforced, natural
Envalior Durethan® BM 40 X H3.0 EF 000000 Nylon 6 (PA6), 40% Glass/Mineral Filled, Dry
Envalior Durethan® BM 40 X H2.0 EF 900116 Nylon 6 (PA6), 40% Glass/Mineral Filled, Dry
Envalior Durethan® BM 40 X H2.0 EF 900116 Nylon 6 (PA6), 40% Glass/Mineral Filled, Conditioned
Envalior Durethan® BM 40 X H2.0 DUS009 901510 Nylon 6 (PA6), 40% Glass/Mineral Reinforced, Conditioned

PLANW9524 / 208289

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.