MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

(Viewing data as-entered. Click here to return)
Ensinger Sintimid™ V-HPHT high purity high temp Polyimide (PI)  (discontinued **)
Categories: Polymer; Thermoplastic; Polyimide, Thermoplastic

Material Notes: SINTIMID™ V polyimide stock shapes provide a superior combination of high temperature and bearing and wear, properties that make it an idea choice for the most demanding applications. SINTIMID™ V is characterized by its long-term thermal stability, outstanding wear resistance, high creep resistance, and strength up to its continuous use temperature of 572°F. Specialty grades containing internal lubricants such as PTFE and graphite are available for applications requiring improved wear resistance and lower coefficients of friction.

  • Superior high temperature characteristics
  • Excellent long-term thermal stability
  • Outstanding bearing and wear properties (at elevated temperatures, SINTIMID™ V formulations offer superior wear rates)
  • Excellent creep resistance
  • High strength and stiffness properties (SINTIMID™ V has a tensile strength of 20,000 psi at room temperature)
  • High purity characteristics (only extremely low levels of extractables and ionic impurities are apparent in SINTIMID™ V)
  • Good chemical resistance (SINTIMID™ V is not attacked by common solvents or fuels and is acceptable for use in contact with many acids)

SINTIMID™ V with its superior physical properties, is ideal for applications in the aerospace, nuclear, automotive, electrical/electronic, and chemical processing industries. It is an excellent candidate for high purity applications in the semiconductor processing industry. Typical components produced from SINTIMID™ V include seals, thrust washers, bushings and wear pads in transportation/off-highway equipment, insulating and support elements in electrical welding and brazing equipment, and wafer-handling components in the harsh environment of semiconductor plasma ovens. Pump and valve seals, vanes, and piston rings are also commonly produced from SINTIMID™ V.

Information Provided by Ensinger Industries, Inc.
Sintimid has been replaced with Tecasint in the Ensinger product line.

Vendors: Ensinger High Performance Plastics withstand severe environments, resist harsh chemicals, and perform well in extreme temperatures. They offer weight savings that have potential to drive lower cost systems.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.35 g/ccASTM D792
Density 0.0488 lb/in³ASTM D792
Water Absorption 1.86 %
@Temperature 22.8 °C,
Time 86400 sec
ASTM D570
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 125ASTM D785
Tensile Strength, Yield 16800 psi
@Temperature 22.8 °C
ASTM D638
Elongation at Break 9.0 %
@Temperature 22.8 °C
ASTM D638
Flexural Strength 25200 psi
@Temperature 22.8 °C
ASTM D790
Flexural Modulus 580000 psi
@Temperature 22.8 °C
ASTM D790
Izod Impact, Notched 0.820 ft-lb/in
@Temperature 22.8 °C
ASTM D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+18 ohm-cmASTM D257
Dielectric Strength 500 V/milASTM D149
 
Thermal PropertiesOriginal ValueComments
CTE, linear 27.0 µin/in-°FASTM D696
Maximum Service Temperature, Air 536 °FLong Term
 626 °FIntermittent
Deflection Temperature at 1.8 MPa (264 psi) 695 °FASTM D648

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Vespel® SP-202 Conductive Polyimide
RTP Company RTP 4299 X 117414 Thermoplastic Polyimide (TPI), Carbon Fiber
DuPont Mobility and Materials VESPEL TP-8054 Polyimide
DuPont Mobility and Materials Vespel® CP-0301 Fiber Compound
DuPont Mobility and Materials Vespel® SCP-50094 Polyimide

PENSIN018 / 92835

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.