MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Outokumpu 4016 Ferritic Stainless Steel
Categories: Metal; Ferrous Metal; Ferritic; Stainless Steel

Material Notes: Fairly good corrosion resistant formable steel in mildly corrosive environments. Oxidation resistant at elevated temperatures (up to ~800°C). Ductile, does not work harden readily, and is well suited for deep drawing and bending.

Applications: Used in a variety of interior applications where material cost and corrosion performance are important factors. Typical applications include:

  • Washing machines
  • Dish-washers
  • Sinks
  • Electrical tie-wire
  • Vine wire
  • Sink rims
  • Counter tops
  • Cooker hoods
  • Refrigerators
  • Tableware
  • Restaurant equipment
  • Indoor cladding
  • Flue-gas ducts

Available in cold rolled narrow strip, bar, and rod forms.

Key Words: EN 1.4016; ASTM 430; JIS SUS 430
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.70 g/ccRT
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 520 MPaOutokumpu Typical, Cold Rolled Strip/Sheet; EN 10002-1
Tensile Strength, Yield 260 MPa
@Strain 0.2 %
EN min., RT; EN 10002-1
 380 MPa
@Strain 0.2 %
Outokumpu Typical, Cold Rolled Strip/Sheet; EN 10002-1
 190 MPa
@Strain 0.2 %,
Temperature 400 °C
EN min.; EN 10002-5
 200 MPa
@Strain 0.2 %,
Temperature 300 °C
EN min.; EN 10002-5
 210 MPa
@Strain 0.2 %,
Temperature 200 °C
EN min.; EN 10002-5
 220 MPa
@Strain 0.2 %,
Temperature 100 °C
EN min.; EN 10002-5
Elongation at Break 25 %Outokumpu Typical, Cold Rolled Strip/Sheet; EN 10002-1
Modulus of Elasticity 220 GPaRT
 195 GPa
@Temperature 400 °C
 205 GPa
@Temperature 300 °C
 210 GPa
@Temperature 200 °C
 215 GPa
@Temperature 100 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000600 ohm-cmRT
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.0 µm/m-°C
@Temperature 100 °C
 10.5 µm/m-°C
@Temperature 300 °C
 10.5 µm/m-°C
@Temperature 400 °C
 11.0 µm/m-°C
@Temperature 500 °C
Specific Heat Capacity 0.460 J/g-°CRT
Thermal Conductivity 25.0 W/m-KRT
 25.0 W/m-K
@Temperature 400 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.040 %
Chromium, Cr 16.5 %
Iron, Fe 83.46 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Outokumpu 4372 Cr-Ni Austenitic Stainless Steel
430 Stainless Steel annealed sheet
ArcelorMittal 51 High formability steel for drawing, Cold rolled
Dura-Bar 65-45-12 Continuously Cast Ductile Iron Bar Stock ASTM A536
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Molded

NOUTOK00 / 18715

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.