Physical Properties | Metric | English | Comments |
---|
Density | 2.84 g/cc | 0.103 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 130 | 130 |
Hardness, Knoop | 163 | 163 |
Hardness, Rockwell A | 49.5 | 49.5 |
Hardness, Rockwell B | 80 | 80 |
Hardness, Vickers | 149 | 149 |
Tensile Strength, Ultimate | >= 400 MPa | >= 58000 psi |
| >= 400 MPa | >= 58000 psi |
| 455 MPa | 66000 psi |
| 30.0 MPa @Temperature 371 °C | 4350 psi @Temperature 700 °F |
| 48.0 MPa @Temperature 316 °C | 6960 psi @Temperature 601 °F |
| 200 MPa @Temperature 260 °C | 29000 psi @Temperature 500 °F |
| 248 MPa @Temperature 204 °C | 36000 psi @Temperature 399 °F |
| 338 MPa @Temperature 149 °C | 49000 psi @Temperature 300 °F |
| 414 MPa @Temperature 100 °C | 60000 psi @Temperature 212 °F |
| 455 MPa @Temperature 24.0 °C | 66000 psi @Temperature 75.2 °F |
| 476 MPa @Temperature -28.0 °C | 69000 psi @Temperature -18.4 °F |
| 490 MPa @Temperature -80.0 °C | 71100 psi @Temperature -112 °F |
| 572 MPa @Temperature -196 °C | 83000 psi @Temperature -321 °F |
| >= 395 MPa @Thickness 127.0 - 152 mm | >= 57300 psi @Thickness 5.001 - 6.00 in |
| >= 405 MPa @Thickness 101.6 - 127 mm | >= 58700 psi @Thickness 4.001 - 5.00 in |
| >= 415 MPa @Thickness 76.23 - 102 mm | >= 60200 psi @Thickness 3.001 - 4.00 in |
| >= 425 MPa @Thickness 6.35 - 50.8 mm | >= 61600 psi @Thickness 0.250 - 2.00 in |
| >= 425 MPa @Thickness 50.83 - 76.2 mm | >= 61600 psi @Thickness 2.001 - 3.00 in |
| >= 395 MPa @Diameter 50.83 - 102 mm | >= 57300 psi @Diameter 2.001 - 4.00 in |
| >= 400 MPa @Diameter 12.7 - 50.8 mm | >= 58000 psi @Diameter 0.500 - 2.00 in |
Tensile Strength, Yield | >= 290 MPa | >= 42100 psi |
| >= 290 MPa | >= 42100 psi |
| 352 MPa | 51000 psi |
| >= 290 MPa @Thickness 127.0 - 152 mm | >= 42100 psi @Thickness 5.001 - 6.00 in |
| >= 295 MPa @Thickness 101.6 - 127 mm | >= 42800 psi @Thickness 4.001 - 5.00 in |
| >= 305 MPa @Thickness 76.23 - 102 mm | >= 44200 psi @Thickness 3.001 - 4.00 in |
| >= 310 MPa @Thickness 50.83 - 76.2 mm | >= 45000 psi @Thickness 2.001 - 3.00 in |
| >= 315 MPa @Thickness 6.35 - 50.8 mm | >= 45700 psi @Thickness 0.250 - 2.00 in |
| >= 270 MPa @Diameter 50.83 - 102 mm | >= 39200 psi @Diameter 2.001 - 4.00 in |
| >= 275 MPa @Diameter 12.7 - 50.8 mm | >= 39900 psi @Diameter 0.500 - 2.00 in |
| 26.0 MPa @Strain 0.2 %, Temperature 371 °C | 3770 psi @Strain 0.2 %, Temperature 700 °F |
| 41.0 MPa @Strain 0.2 %, Temperature 316 °C | 5950 psi @Strain 0.2 %, Temperature 601 °F |
| 159 MPa @Strain 0.2 %, Temperature 260 °C | 23100 psi @Strain 0.2 %, Temperature 500 °F |
| 200 MPa @Strain 0.2 %, Temperature 204 °C | 29000 psi @Strain 0.2 %, Temperature 399 °F |
| 276 MPa @Strain 0.2 %, Temperature 149 °C | 40000 psi @Strain 0.2 %, Temperature 300 °F |
| 324 MPa @Strain 0.2 %, Temperature 100 °C | 47000 psi @Strain 0.2 %, Temperature 212 °F |
| 345 MPa @Strain 0.2 %, Temperature 24.0 °C | 50000 psi @Strain 0.2 %, Temperature 75.2 °F |
| 359 MPa @Strain 0.2 %, Temperature -28.0 °C | 52100 psi @Strain 0.2 %, Temperature -18.4 °F |
| 372 MPa @Strain 0.2 %, Temperature -80.0 °C | 54000 psi @Strain 0.2 %, Temperature -112 °F |
| 421 MPa @Strain 0.2 %, Temperature -196 °C | 61100 psi @Strain 0.2 %, Temperature -321 °F |
Elongation at Break | 6.0 % | 6.0 % |
| 6.0 % | 6.0 % |
| 12 % @Temperature -28.0 °C | 12 % @Temperature -18.4 °F |
| 12 % @Temperature 24.0 °C | 12 % @Temperature 75.2 °F |
| 13 % @Temperature -80.0 °C | 13 % @Temperature -112 °F |
| 15 % @Temperature -196 °C | 15 % @Temperature -321 °F |
| 15 % @Temperature 100 °C | 15 % @Temperature 212 °F |
| 17 % @Temperature 149 °C | 17 % @Temperature 300 °F |
| 20 % @Temperature 204 °C | 20 % @Temperature 399 °F |
| 21 % @Temperature 260 °C | 21 % @Temperature 500 °F |
| 55 % @Temperature 316 °C | 55 % @Temperature 601 °F |
| 75 % @Temperature 371 °C | 75 % @Temperature 700 °F |
| 4.0 % @Thickness 127.0 - 152 mm | 4.0 % @Thickness 5.001 - 6.00 in |
| 5.0 % @Thickness 76.23 - 102 mm | 5.0 % @Thickness 3.001 - 4.00 in |
| 5.0 % @Thickness 101.6 - 127 mm | 5.0 % @Thickness 4.001 - 5.00 in |
| 6.0 % @Thickness 50.83 - 76.2 mm | 6.0 % @Thickness 2.001 - 3.00 in |
| 7.0 - 8.0 % @Thickness 6.35 - 50.8 mm | 7.0 - 8.0 % @Thickness 0.250 - 2.00 in |
| 10 % @Thickness 1.59 mm | 10 % @Thickness 0.0625 in |
| 4.0 % @Diameter 12.7 - 50.8 mm | 4.0 % @Diameter 0.500 - 2.00 in |
| 4.0 % @Diameter 50.83 - 102 mm | 4.0 % @Diameter 2.001 - 4.00 in |
Creep Strength | 11.0 MPa @Temperature 370 °C, Time 3.60e+6 sec | 1600 psi @Temperature 698 °F, Time 1000 hour |
| 13.0 MPa @Temperature 370 °C, Time 3.60e+6 sec | 1890 psi @Temperature 698 °F, Time 1000 hour |
| 13.0 MPa @Temperature 370 °C, Time 360000 sec | 1890 psi @Temperature 698 °F, Time 100 hour |
| 18.0 MPa @Temperature 370 °C, Time 360000 sec | 2610 psi @Temperature 698 °F, Time 100 hour |
| 18.0 MPa @Temperature 370 °C, Time 36000 sec | 2610 psi @Temperature 698 °F, Time 10.0 hour |
| 20.0 MPa @Temperature 370 °C, Time 360000 sec | 2900 psi @Temperature 698 °F, Time 100 hour |
| 23.0 MPa @Temperature 370 °C, Time 36000 sec | 3340 psi @Temperature 698 °F, Time 10.0 hour |
| 23.0 MPa @Temperature 315 °C, Time 3.60e+6 sec | 3340 psi @Temperature 599 °F, Time 1000 hour |
| 27.0 MPa @Temperature 370 °C, Time 36000 sec | 3920 psi @Temperature 698 °F, Time 10.0 hour |
| 28.0 MPa @Temperature 315 °C, Time 3.60e+6 sec | 4060 psi @Temperature 599 °F, Time 1000 hour |
| 30.0 MPa @Temperature 370 °C, Time 36000 sec | 4350 psi @Temperature 698 °F, Time 10.0 hour |
| 32.0 MPa @Temperature 370 °C, Time 3600 sec | 4640 psi @Temperature 698 °F, Time 1.00 hour |
| 38.0 MPa @Temperature 315 °C, Time 3.60e+6 sec | 5510 psi @Temperature 599 °F, Time 1000 hour |
| 38.0 MPa @Temperature 315 °C, Time 360000 sec | 5510 psi @Temperature 599 °F, Time 100 hour |
| 41.0 MPa @Temperature 315 °C, Time 3.60e+6 sec | 5950 psi @Temperature 599 °F, Time 1000 hour |
| 45.0 MPa @Temperature 370 °C, Time 3600 sec | 6530 psi @Temperature 698 °F, Time 1.00 hour |
| 52.0 MPa @Temperature 315 °C, Time 360000 sec | 7540 psi @Temperature 599 °F, Time 100 hour |
| 59.0 MPa @Temperature 370 °C, Time 3600 sec | 8560 psi @Temperature 698 °F, Time 1.00 hour |
| 59.0 MPa @Temperature 260 °C, Time 3.60e+6 sec | 8560 psi @Temperature 500 °F, Time 1000 hour |
| 62.0 MPa @Temperature 370 °C, Time 3600 sec | 8990 psi @Temperature 698 °F, Time 1.00 hour |
| 62.0 MPa @Temperature 315 °C, Time 360000 sec | 8990 psi @Temperature 599 °F, Time 100 hour |
| 62.0 MPa @Temperature 315 °C, Time 36000 sec | 8990 psi @Temperature 599 °F, Time 10.0 hour |
| 66.0 MPa @Temperature 370 °C, Time 360 sec | 9570 psi @Temperature 698 °F, Time 0.100 hour |
| 66.0 MPa @Temperature 370 °C, Time 360 sec | 9570 psi @Temperature 698 °F, Time 0.100 hour |
| 69.0 MPa @Temperature 260 °C, Time 360000 sec | 10000 psi @Temperature 500 °F, Time 100 hour |
| 69.0 MPa @Temperature 260 °C, Time 3.60e+7 sec | 10000 psi @Temperature 500 °F, Time 10000 hour |
| 69.0 MPa @Temperature 315 °C, Time 360000 sec | 10000 psi @Temperature 599 °F, Time 100 hour |
| 69.0 MPa @Temperature 370 °C, Time 360 sec | 10000 psi @Temperature 698 °F, Time 0.100 hour |
| 69.0 MPa @Temperature 370 °C, Time 360 sec | 10000 psi @Temperature 698 °F, Time 0.100 hour |
| 69.0 MPa @Temperature 260 °C, Time 3.60e+6 sec | 10000 psi @Temperature 500 °F, Time 1000 hour |
| 69.0 MPa @Temperature 230 °C, Time 3.60e+6 sec | 10000 psi @Temperature 446 °F, Time 1000 hour |
| 76.0 MPa @Temperature 315 °C, Time 36000 sec | 11000 psi @Temperature 599 °F, Time 10.0 hour |
| 83.0 MPa @Temperature 260 °C, Time 3.60e+6 sec | 12000 psi @Temperature 500 °F, Time 1000 hour |
| 90.0 MPa @Temperature 315 °C, Time 36000 sec | 13100 psi @Temperature 599 °F, Time 10.0 hour |
| 90.0 MPa @Temperature 230 °C, Time 3.60e+6 sec | 13100 psi @Temperature 446 °F, Time 1000 hour |
| 90.0 MPa @Temperature 260 °C, Time 360000 sec | 13100 psi @Temperature 500 °F, Time 100 hour |
| 90.0 MPa @Temperature 205 °C, Time 3.60e+6 sec | 13100 psi @Temperature 401 °F, Time 1000 hour |
| 90.0 MPa @Temperature 230 °C, Time 360000 sec | 13100 psi @Temperature 446 °F, Time 100 hour |
| 90.0 MPa @Temperature 260 °C, Time 36000 sec | 13100 psi @Temperature 500 °F, Time 10.0 hour |
| 90.0 MPa @Temperature 315 °C, Time 3600 sec | 13100 psi @Temperature 599 °F, Time 1.00 hour |
| 97.0 MPa @Temperature 230 °C, Time 3.60e+7 sec | 14100 psi @Temperature 446 °F, Time 10000 hour |
| 97.0 MPa @Temperature 260 °C, Time 3.60e+6 sec | 14100 psi @Temperature 500 °F, Time 1000 hour |
| 97.0 MPa @Temperature 315 °C, Time 36000 sec | 14100 psi @Temperature 599 °F, Time 10.0 hour |
| 97.0 MPa @Temperature 230 °C, Time 3.60e+7 sec | 14100 psi @Temperature 446 °F, Time 10000 hour |
| 105 MPa @Temperature 315 °C, Time 3600 sec | 15200 psi @Temperature 599 °F, Time 1.00 hour |
| 105 MPa @Temperature 175 °C, Time 3.60e+6 sec | 15200 psi @Temperature 347 °F, Time 1000 hour |
| 110 MPa @Temperature 230 °C, Time 3.60e+6 sec | 16000 psi @Temperature 446 °F, Time 1000 hour |
| 110 MPa @Temperature 260 °C, Time 360000 sec | 16000 psi @Temperature 500 °F, Time 100 hour |
| 110 MPa @Temperature 315 °C, Time 3600 sec | 16000 psi @Temperature 599 °F, Time 1.00 hour |
| 110 MPa @Temperature 230 °C, Time 360000 sec | 16000 psi @Temperature 446 °F, Time 100 hour |
| 110 MPa @Temperature 260 °C, Time 36000 sec | 16000 psi @Temperature 500 °F, Time 10.0 hour |
| 110 MPa @Temperature 205 °C, Time 360000 sec | 16000 psi @Temperature 401 °F, Time 100 hour |
| 110 MPa @Temperature 230 °C, Time 36000 sec | 16000 psi @Temperature 446 °F, Time 10.0 hour |
| 110 MPa @Temperature 315 °C, Time 360 sec | 16000 psi @Temperature 599 °F, Time 0.100 hour |
| 115 MPa @Temperature 230 °C, Time 3.60e+6 sec | 16700 psi @Temperature 446 °F, Time 1000 hour |
| 115 MPa @Temperature 315 °C, Time 3600 sec | 16700 psi @Temperature 599 °F, Time 1.00 hour |
| 115 MPa @Temperature 205 °C, Time 3.60e+6 sec | 16700 psi @Temperature 401 °F, Time 1000 hour |
| 115 MPa @Temperature 315 °C, Time 360 sec | 16700 psi @Temperature 599 °F, Time 0.100 hour |
| 115 MPa @Temperature 260 °C, Time 3600 sec | 16700 psi @Temperature 500 °F, Time 1.00 hour |
| 125 MPa @Temperature 205 °C, Time 3.60e+7 sec | 18100 psi @Temperature 401 °F, Time 10000 hour |
| 125 MPa @Temperature 260 °C, Time 360000 sec | 18100 psi @Temperature 500 °F, Time 100 hour |
| 125 MPa @Temperature 315 °C, Time 360 sec | 18100 psi @Temperature 599 °F, Time 0.100 hour |
| 125 MPa @Temperature 205 °C, Time 3.60e+6 sec | 18100 psi @Temperature 401 °F, Time 1000 hour |
| 125 MPa @Temperature 315 °C, Time 360 sec | 18100 psi @Temperature 599 °F, Time 0.100 hour |
| 130 MPa @Temperature 230 °C, Time 360000 sec | 18900 psi @Temperature 446 °F, Time 100 hour |
| 130 MPa @Temperature 260 °C, Time 36000 sec | 18900 psi @Temperature 500 °F, Time 10.0 hour |
| 130 MPa @Temperature 205 °C, Time 360000 sec | 18900 psi @Temperature 401 °F, Time 100 hour |
| 130 MPa @Temperature 230 °C, Time 36000 sec | 18900 psi @Temperature 446 °F, Time 10.0 hour |
| 130 MPa @Temperature 175 °C, Time 360000 sec | 18900 psi @Temperature 347 °F, Time 100 hour |
| 130 MPa @Temperature 205 °C, Time 36000 sec | 18900 psi @Temperature 401 °F, Time 10.0 hour |
| 140 MPa @Temperature 205 °C, Time 3.60e+6 sec | 20300 psi @Temperature 401 °F, Time 1000 hour |
| 140 MPa @Temperature 230 °C, Time 360000 sec | 20300 psi @Temperature 446 °F, Time 100 hour |
| 140 MPa @Temperature 260 °C, Time 36000 sec | 20300 psi @Temperature 500 °F, Time 10.0 hour |
| 140 MPa @Temperature 175 °C, Time 3.60e+6 sec | 20300 psi @Temperature 347 °F, Time 1000 hour |
| 140 MPa @Temperature 260 °C, Time 3600 sec | 20300 psi @Temperature 500 °F, Time 1.00 hour |
| 140 MPa @Temperature 230 °C, Time 3600 sec | 20300 psi @Temperature 446 °F, Time 1.00 hour |
| 145 MPa @Temperature 260 °C, Time 360 sec | 21000 psi @Temperature 500 °F, Time 0.100 hour |
| 150 MPa @Temperature 205 °C, Time 360000 sec | 21800 psi @Temperature 401 °F, Time 100 hour |
| 150 MPa @Temperature 230 °C, Time 36000 sec | 21800 psi @Temperature 446 °F, Time 10.0 hour |
| 150 MPa @Temperature 260 °C, Time 3600 sec | 21800 psi @Temperature 500 °F, Time 1.00 hour |
| 150 MPa @Temperature 205 °C, Time 36000 sec | 21800 psi @Temperature 401 °F, Time 10.0 hour |
| 150 MPa @Temperature 230 °C, Time 3600 sec | 21800 psi @Temperature 446 °F, Time 1.00 hour |
| 150 MPa @Temperature 150 °C, Time 3.60e+6 sec | 21800 psi @Temperature 302 °F, Time 1000 hour |
| 160 MPa @Temperature 230 °C, Time 36000 sec | 23200 psi @Temperature 446 °F, Time 10.0 hour |
| 160 MPa @Temperature 260 °C, Time 3600 sec | 23200 psi @Temperature 500 °F, Time 1.00 hour |
| 160 MPa @Temperature 175 °C, Time 3.60e+6 sec | 23200 psi @Temperature 347 °F, Time 1000 hour |
| 160 MPa @Temperature 175 °C, Time 360000 sec | 23200 psi @Temperature 347 °F, Time 100 hour |
| 160 MPa @Temperature 260 °C, Time 360 sec | 23200 psi @Temperature 500 °F, Time 0.100 hour |
| 160 MPa @Temperature 205 °C, Time 3600 sec | 23200 psi @Temperature 401 °F, Time 1.00 hour |
| 165 MPa @Temperature 205 °C, Time 360000 sec | 23900 psi @Temperature 401 °F, Time 100 hour |
| 165 MPa @Temperature 260 °C, Time 360 sec | 23900 psi @Temperature 500 °F, Time 0.100 hour |
| 165 MPa @Temperature 150 °C, Time 3.60e+6 sec | 23900 psi @Temperature 302 °F, Time 1000 hour |
| 165 MPa @Temperature 175 °C, Time 36000 sec | 23900 psi @Temperature 347 °F, Time 10.0 hour |
| 165 MPa @Temperature 230 °C, Time 360 sec | 23900 psi @Temperature 446 °F, Time 0.100 hour |
| 170 MPa @Temperature 175 °C, Time 3.60e+6 sec | 24700 psi @Temperature 347 °F, Time 1000 hour |
| 170 MPa @Temperature 260 °C, Time 360 sec | 24700 psi @Temperature 500 °F, Time 0.100 hour |
| 170 MPa @Temperature 230 °C, Time 3600 sec | 24700 psi @Temperature 446 °F, Time 1.00 hour |
| 170 MPa @Temperature 150 °C, Time 360000 sec | 24700 psi @Temperature 302 °F, Time 100 hour |
| 180 MPa @Temperature 205 °C, Time 36000 sec | 26100 psi @Temperature 401 °F, Time 10.0 hour |
| 180 MPa @Temperature 205 °C, Time 3600 sec | 26100 psi @Temperature 401 °F, Time 1.00 hour |
| 180 MPa @Temperature 230 °C, Time 360 sec | 26100 psi @Temperature 446 °F, Time 0.100 hour |
| 185 MPa @Temperature 230 °C, Time 3600 sec | 26800 psi @Temperature 446 °F, Time 1.00 hour |
| 185 MPa @Temperature 175 °C, Time 360000 sec | 26800 psi @Temperature 347 °F, Time 100 hour |
| 195 MPa @Temperature 205 °C, Time 36000 sec | 28300 psi @Temperature 401 °F, Time 10.0 hour |
| 195 MPa @Temperature 175 °C, Time 36000 sec | 28300 psi @Temperature 347 °F, Time 10.0 hour |
| 195 MPa @Temperature 205 °C, Time 360 sec | 28300 psi @Temperature 401 °F, Time 0.100 hour |
| 200 MPa @Temperature 175 °C, Time 360000 sec | 29000 psi @Temperature 347 °F, Time 100 hour |
| 200 MPa @Temperature 150 °C, Time 3.60e+6 sec | 29000 psi @Temperature 302 °F, Time 1000 hour |
| 200 MPa @Temperature 230 °C, Time 360 sec | 29000 psi @Temperature 446 °F, Time 0.100 hour |
| 200 MPa @Temperature 150 °C, Time 360000 sec | 29000 psi @Temperature 302 °F, Time 100 hour |
| 200 MPa @Temperature 175 °C, Time 3600 sec | 29000 psi @Temperature 347 °F, Time 1.00 hour |
| 205 MPa @Temperature 230 °C, Time 360 sec | 29700 psi @Temperature 446 °F, Time 0.100 hour |
| 205 MPa @Temperature 205 °C, Time 3600 sec | 29700 psi @Temperature 401 °F, Time 1.00 hour |
| 205 MPa @Temperature 150 °C, Time 36000 sec | 29700 psi @Temperature 302 °F, Time 10.0 hour |
| 215 MPa @Temperature 175 °C, Time 36000 sec | 31200 psi @Temperature 347 °F, Time 10.0 hour |
| 215 MPa @Temperature 205 °C, Time 360 sec | 31200 psi @Temperature 401 °F, Time 0.100 hour |
| 220 MPa @Temperature 150 °C, Time 3.60e+6 sec | 31900 psi @Temperature 302 °F, Time 1000 hour |
| 220 MPa @Temperature 205 °C, Time 3600 sec | 31900 psi @Temperature 401 °F, Time 1.00 hour |
| 220 MPa @Temperature 175 °C, Time 3600 sec | 31900 psi @Temperature 347 °F, Time 1.00 hour |
| 230 MPa @Temperature 175 °C, Time 36000 sec | 33400 psi @Temperature 347 °F, Time 10.0 hour |
| 230 MPa @Temperature 175 °C, Time 360 sec | 33400 psi @Temperature 347 °F, Time 0.100 hour |
| 235 MPa @Temperature 150 °C, Time 360000 sec | 34100 psi @Temperature 302 °F, Time 100 hour |
| 235 MPa @Temperature 205 °C, Time 360 sec | 34100 psi @Temperature 401 °F, Time 0.100 hour |
| 235 MPa @Temperature 150 °C, Time 36000 sec | 34100 psi @Temperature 302 °F, Time 10.0 hour |
| 235 MPa @Temperature 150 °C, Time 3600 sec | 34100 psi @Temperature 302 °F, Time 1.00 hour |
| 240 MPa @Temperature 205 °C, Time 360 sec | 34800 psi @Temperature 401 °F, Time 0.100 hour |
| 240 MPa @Temperature 175 °C, Time 3600 sec | 34800 psi @Temperature 347 °F, Time 1.00 hour |
| 250 MPa @Temperature 150 °C, Time 360000 sec | 36300 psi @Temperature 302 °F, Time 100 hour |
| 250 MPa @Temperature 175 °C, Time 360 sec | 36300 psi @Temperature 347 °F, Time 0.100 hour |
| 255 MPa @Temperature 175 °C, Time 3600 sec | 37000 psi @Temperature 347 °F, Time 1.00 hour |
| 255 MPa @Temperature 150 °C, Time 36000 sec | 37000 psi @Temperature 302 °F, Time 10.0 hour |
| 255 MPa @Temperature 150 °C, Time 3600 sec | 37000 psi @Temperature 302 °F, Time 1.00 hour |
| 260 MPa @Temperature 175 °C, Time 360 sec | 37700 psi @Temperature 347 °F, Time 0.100 hour |
| 260 MPa @Temperature 100 °C, Time 3.60e+6 sec | 37700 psi @Temperature 212 °F, Time 1000 hour |
| 260 MPa @Temperature 150 °C, Time 360 sec | 37700 psi @Temperature 302 °F, Time 0.100 hour |
| 270 MPa @Temperature 150 °C, Time 36000 sec | 39200 psi @Temperature 302 °F, Time 10.0 hour |
| 270 MPa @Temperature 100 °C, Time 3.60e+6 sec | 39200 psi @Temperature 212 °F, Time 1000 hour |
| 270 MPa @Temperature 100 °C, Time 360000 sec | 39200 psi @Temperature 212 °F, Time 100 hour |
| 275 MPa @Temperature 175 °C, Time 360 sec | 39900 psi @Temperature 347 °F, Time 0.100 hour |
| 275 MPa @Temperature 150 °C, Time 3600 sec | 39900 psi @Temperature 302 °F, Time 1.00 hour |
| 275 MPa @Temperature 100 °C, Time 360000 sec | 39900 psi @Temperature 212 °F, Time 100 hour |
| 275 MPa @Temperature 150 °C, Time 360 sec | 39900 psi @Temperature 302 °F, Time 0.100 hour |
| 275 MPa @Temperature 100 °C, Time 36000 sec | 39900 psi @Temperature 212 °F, Time 10.0 hour |
| 285 MPa @Temperature 100 °C, Time 3.60e+6 sec | 41300 psi @Temperature 212 °F, Time 1000 hour |
| 285 MPa @Temperature 100 °C, Time 3600 sec | 41300 psi @Temperature 212 °F, Time 1.00 hour |
| 290 MPa @Temperature 150 °C, Time 3600 sec | 42100 psi @Temperature 302 °F, Time 1.00 hour |
| 290 MPa @Temperature 100 °C, Time 36000 sec | 42100 psi @Temperature 212 °F, Time 10.0 hour |
| 295 MPa @Temperature 100 °C, Time 3.60e+6 sec | 42800 psi @Temperature 212 °F, Time 1000 hour |
| 295 MPa @Temperature 100 °C, Time 360000 sec | 42800 psi @Temperature 212 °F, Time 100 hour |
| 295 MPa @Temperature 150 °C, Time 360 sec | 42800 psi @Temperature 302 °F, Time 0.100 hour |
| 305 MPa @Temperature 150 °C, Time 360 sec | 44200 psi @Temperature 302 °F, Time 0.100 hour |
| 305 MPa @Temperature 100 °C, Time 3600 sec | 44200 psi @Temperature 212 °F, Time 1.00 hour |
| 305 MPa @Temperature 100 °C, Time 360 sec | 44200 psi @Temperature 212 °F, Time 0.100 hour |
| 310 MPa @Temperature 100 °C, Time 360000 sec | 45000 psi @Temperature 212 °F, Time 100 hour |
| 310 MPa @Temperature 100 °C, Time 36000 sec | 45000 psi @Temperature 212 °F, Time 10.0 hour |
| 315 MPa @Temperature 100 °C, Time 360 sec | 45700 psi @Temperature 212 °F, Time 0.100 hour |
| 315 MPa @Temperature 24.0 °C, Time 3.60e+6 sec | 45700 psi @Temperature 75.2 °F, Time 1000 hour |
| 325 MPa @Temperature 100 °C, Time 36000 sec | 47100 psi @Temperature 212 °F, Time 10.0 hour |
| 325 MPa @Temperature 100 °C, Time 3600 sec | 47100 psi @Temperature 212 °F, Time 1.00 hour |
| 325 MPa @Temperature 24.0 °C, Time 360000 sec | 47100 psi @Temperature 75.2 °F, Time 100 hour |
| 330 MPa @Temperature 24.0 °C, Time 3.60e+6 sec | 47900 psi @Temperature 75.2 °F, Time 1000 hour |
| 330 MPa @Temperature 24.0 °C, Time 36000 sec | 47900 psi @Temperature 75.2 °F, Time 10.0 hour |
| 340 MPa @Temperature 100 °C, Time 3600 sec | 49300 psi @Temperature 212 °F, Time 1.00 hour |
| 340 MPa @Temperature 100 °C, Time 360 sec | 49300 psi @Temperature 212 °F, Time 0.100 hour |
| 340 MPa @Temperature 24.0 °C, Time 360000 sec | 49300 psi @Temperature 75.2 °F, Time 100 hour |
| 345 MPa @Temperature 24.0 °C, Time 36000 sec | 50000 psi @Temperature 75.2 °F, Time 10.0 hour |
| 345 MPa @Temperature 24.0 °C, Time 3600 sec | 50000 psi @Temperature 75.2 °F, Time 1.00 hour |
| 350 MPa @Temperature 24.0 °C, Time 3.60e+6 sec | 50800 psi @Temperature 75.2 °F, Time 1000 hour |
| 350 MPa @Temperature 24.0 °C, Time 360 sec | 50800 psi @Temperature 75.2 °F, Time 0.100 hour |
| 360 MPa @Temperature 100 °C, Time 360 sec | 52200 psi @Temperature 212 °F, Time 0.100 hour |
| 360 MPa @Temperature 24.0 °C, Time 360000 sec | 52200 psi @Temperature 75.2 °F, Time 100 hour |
| 360 MPa @Temperature 24.0 °C, Time 3600 sec | 52200 psi @Temperature 75.2 °F, Time 1.00 hour |
| 365 MPa @Temperature 24.0 °C, Time 3.60e+6 sec | 52900 psi @Temperature 75.2 °F, Time 1000 hour |
| 365 MPa @Temperature 24.0 °C, Time 36000 sec | 52900 psi @Temperature 75.2 °F, Time 10.0 hour |
| 365 MPa @Temperature 24.0 °C, Time 360 sec | 52900 psi @Temperature 75.2 °F, Time 0.100 hour |
| 380 MPa @Temperature 24.0 °C, Time 360000 sec | 55100 psi @Temperature 75.2 °F, Time 100 hour |
| 385 MPa @Temperature 24.0 °C, Time 3600 sec | 55800 psi @Temperature 75.2 °F, Time 1.00 hour |
| 400 MPa @Temperature 24.0 °C, Time 36000 sec | 58000 psi @Temperature 75.2 °F, Time 10.0 hour |
| 415 MPa @Temperature 24.0 °C, Time 360 sec | 60200 psi @Temperature 75.2 °F, Time 0.100 hour |
| 420 MPa @Temperature 24.0 °C, Time 3600 sec | 60900 psi @Temperature 75.2 °F, Time 1.00 hour |
| 435 MPa @Temperature 24.0 °C, Time 360 sec | 63100 psi @Temperature 75.2 °F, Time 0.100 hour |
Rupture Strength | 14.0 MPa @Temperature 370 °C, Time 3.60e+6 sec | 2030 psi @Temperature 698 °F, Time 1000 hour |
| 22.0 MPa @Temperature 315 °C, Time 3.60e+7 sec | 3190 psi @Temperature 599 °F, Time 10000 hour |
| 22.0 MPa @Temperature 370 °C, Time 360000 sec | 3190 psi @Temperature 698 °F, Time 100 hour |
| 32.0 MPa @Temperature 370 °C, Time 36000 sec | 4640 psi @Temperature 698 °F, Time 10.0 hour |
| 41.0 MPa @Temperature 315 °C, Time 3.60e+6 sec | 5950 psi @Temperature 599 °F, Time 1000 hour |
| 45.0 MPa @Temperature 260 °C, Time 3.60e+8 sec | 6530 psi @Temperature 500 °F, Time 100000 hour |
| 62.0 MPa @Temperature 370 °C, Time 3600 sec | 8990 psi @Temperature 698 °F, Time 1.00 hour |
| 66.0 MPa @Temperature 230 °C, Time 3.60e+8 sec | 9570 psi @Temperature 446 °F, Time 100000 hour |
| 69.0 MPa @Temperature 260 °C, Time 3.60e+7 sec | 10000 psi @Temperature 500 °F, Time 10000 hour |
| 69.0 MPa @Temperature 315 °C, Time 360000 sec | 10000 psi @Temperature 599 °F, Time 100 hour |
| 69.0 MPa @Temperature 370 °C, Time 360 sec | 10000 psi @Temperature 698 °F, Time 0.100 hour |
| 97.0 MPa @Temperature 205 °C, Time 3.60e+8 sec | 14100 psi @Temperature 401 °F, Time 100000 hour |
| 97.0 MPa @Temperature 230 °C, Time 3.60e+7 sec | 14100 psi @Temperature 446 °F, Time 10000 hour |
| 105 MPa @Temperature 260 °C, Time 3.60e+6 sec | 15200 psi @Temperature 500 °F, Time 1000 hour |
| 105 MPa @Temperature 315 °C, Time 36000 sec | 15200 psi @Temperature 599 °F, Time 10.0 hour |
| 115 MPa @Temperature 315 °C, Time 3600 sec | 16700 psi @Temperature 599 °F, Time 1.00 hour |
| 125 MPa @Temperature 205 °C, Time 3.60e+7 sec | 18100 psi @Temperature 401 °F, Time 10000 hour |
| 125 MPa @Temperature 230 °C, Time 3.60e+6 sec | 18100 psi @Temperature 446 °F, Time 1000 hour |
| 130 MPa @Temperature 175 °C, Time 3.60e+8 sec | 18900 psi @Temperature 347 °F, Time 100000 hour |
| 130 MPa @Temperature 260 °C, Time 360000 sec | 18900 psi @Temperature 500 °F, Time 100 hour |
| 130 MPa @Temperature 315 °C, Time 360 sec | 18900 psi @Temperature 599 °F, Time 0.100 hour |
| 150 MPa @Temperature 205 °C, Time 3.60e+6 sec | 21800 psi @Temperature 401 °F, Time 1000 hour |
| 150 MPa @Temperature 230 °C, Time 360000 sec | 21800 psi @Temperature 446 °F, Time 100 hour |
| 150 MPa @Temperature 260 °C, Time 36000 sec | 21800 psi @Temperature 500 °F, Time 10.0 hour |
| 160 MPa @Temperature 175 °C, Time 3.60e+7 sec | 23200 psi @Temperature 347 °F, Time 10000 hour |
| 165 MPa @Temperature 260 °C, Time 3600 sec | 23900 psi @Temperature 500 °F, Time 1.00 hour |
| 170 MPa @Temperature 150 °C, Time 3.60e+8 sec | 24700 psi @Temperature 302 °F, Time 100000 hour |
| 170 MPa @Temperature 230 °C, Time 36000 sec | 24700 psi @Temperature 446 °F, Time 10.0 hour |
| 180 MPa @Temperature 205 °C, Time 360000 sec | 26100 psi @Temperature 401 °F, Time 100 hour |
| 180 MPa @Temperature 260 °C, Time 360 sec | 26100 psi @Temperature 500 °F, Time 0.100 hour |
| 185 MPa @Temperature 175 °C, Time 3.60e+6 sec | 26800 psi @Temperature 347 °F, Time 1000 hour |
| 200 MPa @Temperature 230 °C, Time 3600 sec | 29000 psi @Temperature 446 °F, Time 1.00 hour |
| 205 MPa @Temperature 150 °C, Time 3.60e+7 sec | 29700 psi @Temperature 302 °F, Time 10000 hour |
| 205 MPa @Temperature 205 °C, Time 36000 sec | 29700 psi @Temperature 401 °F, Time 10.0 hour |
| 220 MPa @Temperature 175 °C, Time 360000 sec | 31900 psi @Temperature 347 °F, Time 100 hour |
| 230 MPa @Temperature 230 °C, Time 360 sec | 33400 psi @Temperature 446 °F, Time 0.100 hour |
| 235 MPa @Temperature 150 °C, Time 3.60e+6 sec | 34100 psi @Temperature 302 °F, Time 1000 hour |
| 235 MPa @Temperature 205 °C, Time 3600 sec | 34100 psi @Temperature 401 °F, Time 1.00 hour |
| 250 MPa @Temperature 175 °C, Time 36000 sec | 36300 psi @Temperature 347 °F, Time 10.0 hour |
| 260 MPa @Temperature 150 °C, Time 360000 sec | 37700 psi @Temperature 302 °F, Time 100 hour |
| 270 MPa @Temperature 205 °C, Time 360 sec | 39200 psi @Temperature 401 °F, Time 0.100 hour |
| 275 MPa @Temperature 175 °C, Time 3600 sec | 39900 psi @Temperature 347 °F, Time 1.00 hour |
| 290 MPa @Temperature 150 °C, Time 36000 sec | 42100 psi @Temperature 302 °F, Time 10.0 hour |
| 305 MPa @Temperature 175 °C, Time 360 sec | 44200 psi @Temperature 347 °F, Time 0.100 hour |
| 315 MPa @Temperature 100 °C, Time 3.60e+6 sec | 45700 psi @Temperature 212 °F, Time 1000 hour |
| 315 MPa @Temperature 150 °C, Time 3600 sec | 45700 psi @Temperature 302 °F, Time 1.00 hour |
| 330 MPa @Temperature 100 °C, Time 360000 sec | 47900 psi @Temperature 212 °F, Time 100 hour |
| 340 MPa @Temperature 150 °C, Time 360 sec | 49300 psi @Temperature 302 °F, Time 0.100 hour |
| 350 MPa @Temperature 100 °C, Time 36000 sec | 50800 psi @Temperature 212 °F, Time 10.0 hour |
| 370 MPa @Temperature 100 °C, Time 3600 sec | 53700 psi @Temperature 212 °F, Time 1.00 hour |
| 395 MPa @Temperature 100 °C, Time 360 sec | 57300 psi @Temperature 212 °F, Time 0.100 hour |
| 420 MPa @Temperature 24.0 °C, Time 3.60e+6 sec | 60900 psi @Temperature 75.2 °F, Time 1000 hour |
| 425 MPa @Temperature 24.0 °C, Time 360000 sec | 61600 psi @Temperature 75.2 °F, Time 100 hour |
| 435 MPa @Temperature 24.0 °C, Time 36000 sec | 63100 psi @Temperature 75.2 °F, Time 10.0 hour |
| 450 MPa @Temperature 24.0 °C, Time 3600 sec | 65300 psi @Temperature 75.2 °F, Time 1.00 hour |
| 455 MPa @Temperature 24.0 °C, Time 360 sec | 66000 psi @Temperature 75.2 °F, Time 0.100 hour |
Modulus of Elasticity | 73.1 GPa | 10600 ksi |
Poissons Ratio | 0.33 | 0.33 |
Fatigue Strength | 103 MPa @# of Cycles 5.00e+8 | 15000 psi @# of Cycles 5.00e+8 |
Shear Modulus | 27.0 GPa | 3920 ksi |
Shear Strength | 285 MPa | 41300 psi |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.00000570 ohm-cm | 0.00000570 ohm-cm |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 20.8 µm/m-°C @Temperature -50.0 - 20.0 °C | 11.6 µin/in-°F @Temperature -58.0 - 68.0 °F |
| 22.3 µm/m-°C @Temperature 20.0 - 100 °C | 12.4 µin/in-°F @Temperature 68.0 - 212 °F |
| 22.5 µm/m-°C @Temperature 20.0 - 100 °C | 12.5 µin/in-°F @Temperature 68.0 - 212 °F |
| 23.4 µm/m-°C @Temperature 20.0 - 200 °C | 13.0 µin/in-°F @Temperature 68.0 - 392 °F |
| 24.1 µm/m-°C @Temperature 20.0 - 300 °C | 13.4 µin/in-°F @Temperature 68.0 - 572 °F |
| 24.4 µm/m-°C @Temperature 20.0 - 300 °C | 13.6 µin/in-°F @Temperature 68.0 - 572 °F |
Specific Heat Capacity | 0.864 J/g-°C | 0.207 BTU/lb-°F |
Thermal Conductivity | 120 W/m-K | 833 BTU-in/hr-ft²-°F |
Melting Point | 543 - 643 °C | 1010 - 1190 °F |
Solidus | 543 °C | 1010 °F |
Liquidus | 643 °C | 1190 °F |
|
Processing Properties | Metric | English | Comments |
---|
Annealing Temperature | 413 °C | 775 °F |
Solution Temperature | 535 °C | 995 °F |
Aging Temperature | 163 - 191 °C | 325 - 375 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Aluminum, Al | 91.5 - 93.8 % | 91.5 - 93.8 % |
Copper, Cu | 5.8 - 6.8 % | 5.8 - 6.8 % |
Iron, Fe | <= 0.30 % | <= 0.30 % |
Magnesium, Mg | <= 0.02 % | <= 0.02 % |
Manganese, Mn | 0.20 - 0.40 % | 0.20 - 0.40 % |
Other, each | <= 0.05 % | <= 0.05 % |
Other, total | <= 0.15 % | <= 0.15 % |
Silicon, Si | <= 0.20 % | <= 0.20 % |
Titanium, Ti | 0.02 - 0.10 % | 0.02 - 0.10 % |
Vanadium, V | 0.05 - 0.15 % | 0.05 - 0.15 % |
Zinc, Zn | <= 0.10 % | <= 0.10 % |
Zirconium, Zr | 0.10 - 0.25 % | 0.10 - 0.25 % |