MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Silver-Magnesium-Nickel Alloy Strip (Ag-0.25Ni-0.25Mg), Soft Temper
Categories: Metal; Nonferrous Metal; Precious Metal; Silver Alloy

Material Notes: This alloy can be strengthened by oxidation, typically after fabrication. The Mg oxidizes and creates tiny MgO particles to provide dispersion strengthening.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 10.49 g/cc(pure silver)
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 250 MPa
Tensile Strength, Yield 130 MPa
Elongation at Break 28 %
Reduction of Area 0.0 %
Modulus of Elasticity 83.0 GPaTypical of oxidized sample
 
Thermal PropertiesOriginal ValueComments
CTE, linear 19.7 µm/m-°C
@Temperature 20.0 - 100 °C
Estimated from pure Ag
 20.0 µm/m-°C
@Temperature 20.0 - 250 °C
Estimated from pure Ag
 20.6 µm/m-°C
@Temperature 20.0 - 500 °C
Estimated from pure Ag
Specific Heat Capacity 0.230 J/g-°CEstimated from pure Ag.
 
Component Elements PropertiesOriginal ValueComments
Magnesium, Mg <= 0.25 %
Nickel, Ni 0.25 %
Silver, Ag 95.5 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Silver-Copper Eutectic Alloy (72Ag-28Cu; UNS P07720; AWS BAg-8), Cold Drawn then Annealed at 250°C (480°F)
90Ag-10Pd Alloy, Annealed
99Ag-1Pd Alloy, Annealed
97Ag-3Pd Alloy, Annealed
50Ag-50Pd Alloy, Annealed

MPAgM0 / 12515

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.