MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
TTC Taita TAITALAC® 1400 SAN
Categories: Polymer; Thermoplastic; SAN Polymer; Styrene Acrylonitrile (SAN), Molded

Material Notes: Characteristics:
  • Injection
  • Compounding
Applications:
  • Glass fiber compounding
  • Alloy compoundingInformation provided by Taita Chemical Company, Limited
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.03 g/ccISO 1183
Moisture Absorption at Equilibrium <= 0.30 %C/50% RH; ISO 62
Linear Mold Shrinkage <= 0.0040 cm/cm60×60×2mm Sflow; ISO 294-4
Melt Flow 2.6 g/10 min
@Load 10.0 kg,
Temperature 220 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 83ISO 2039-2
Tensile Strength at Break 69.0 MPa50 mm/min; ISO 527
Tensile Strength, Yield 74.0 MPa50 mm/min; ISO 527
Elongation at Break 30 %50 mm/min; ISO 527
Flexural Yield Strength 107 MPa2.0 mm/min; ISO 178
Flexural Modulus 2900 MPa2.0 mm/min; ISO 178
Izod Impact, Notched (ISO) 1.80 kJ/m²ISO 180/1A
Charpy Impact, Notched 2.80 kJ/m²ISO 179/1A
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 91.0 °Cunannealing; ISO 75
Vicat Softening Point 103 °C
@Load 1.00 kg
50°C/hr; ISO 306
Flammability, UL94 HB
@Thickness 1.59 mm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTTC018 / 281538

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.