MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
AISI 4130 Steel, water quenched 855°C (1570°F), 540°C (1000°F) temper, 25 mm (1 in.) round
Categories: Metal; Ferrous Metal; Alloy Steel; AISI 4000 Series Steel; Low Alloy Steel; Carbon Steel; Medium Carbon Steel

Material Notes: A very common general purpose grade of medium carbon, Cr-Mo steel. Flexibility afforded by heat treatment options allows it to attain a range of toughness and strength values. Good hardenability, strength, wear resistance, toughness, and ductility.

As quenched hardness: 51 HRC surface, 50 HRC 1/2 radius, 44 HRC center

Key Words: alloy steels, UNS G41300, AMS 6350, AMS 6356, AMS 6360, AMS 6361, AMS 6372, AMS 6370, AMS 6371, AMS 6373, ASTM A322, ASTM A331, ASTM A505, ASTM A513, ASTM A519, ASTM A646, JIS SCM 2, JIS SCCrM 1, SS14 2225 (Sweden), B.S. CDS 110 (UK), MIL SPEC MIL-S-16974, SAE J404, SAE J412, SAE J770, DIN 1.7218, AFNOR 25 CD 4 (France), MIL-S-6758 (flat and round bar), MIS-S-18729 ANN and NORM (sheet and plate), QQS-624 (round bar)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.85 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 293
Hardness, Knoop 319Converted from Brinell
Hardness, Rockwell B 99Converted from Brinell
Hardness, Rockwell C 31Converted from Brinell
Hardness, Vickers 309Converted from Brinell
Tensile Strength, Ultimate 993 MPa
Tensile Strength, Yield 896 MPa
Elongation at Break 18.5 %in 50 mm
Reduction of Area 61.8 %
Modulus of Elasticity 205 GPaTypical for steel
Bulk Modulus 160 GPaTypical for steel
Poissons Ratio 0.29Calculated
Machinability 70 %annealed and cold drawn. Based on 100% machinability for AISI 1212 steel.
Shear Modulus 80.0 GPaTypical for steel
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000223 ohm-cm
@Temperature 20.0 °C
specimen hardened and tempered
 0.0000271 ohm-cm
@Temperature 100 °C
specimen hardened and tempered
 0.0000342 ohm-cm
@Temperature 200 °C
specimen hardened and tempered
 0.0000529 ohm-cm
@Temperature 400 °C
specimen hardened and tempered
 0.0000786 ohm-cm
@Temperature 600 °C
specimen hardened and tempered
 0.0001103 ohm-cm
@Temperature 800 °C
specimen hardened and tempered
 0.0001171 ohm-cm
@Temperature 1000 °C
specimen hardened and tempered
 0.0001222 ohm-cm
@Temperature 1200 °C
specimen hardened and tempered
 
Thermal PropertiesOriginal ValueComments
Specific Heat Capacity 0.477 J/g-°C
@Temperature >=100 °C
 0.523 J/g-°C
@Temperature 150 - 200 °C
 0.837 J/g-°C
@Temperature 750 - 800 °C
Thermal Conductivity 30.1 W/m-K
@Temperature 1200 °C
 40.7 W/m-K
@Temperature 300 °C
 42.7 W/m-K
@Temperature 100 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.28 - 0.33 %
Chromium, Cr 0.80 - 1.1 %
Iron, Fe 97.03 - 98.22 %As remainder
Manganese, Mn 0.40 - 0.60 %
Molybdenum, Mo 0.15 - 0.25 %
Phosphorus, P <= 0.035 %
Silicon, Si 0.15 - 0.30 %
Sulfur, S <= 0.040 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 4130 Steel, water quenched 855°C (1570°F), 480°C (900°F) temper, 25 mm (1 in.) round
AISI 4130 Steel, water quenched 855°C (1570°F), 595°C (1100°F) temper, 25 mm (1 in.) round
AISI 4130 Steel, normalized at 870°C (1600°F), air cooled, 25 mm (1 in.) round
AISI 4130 Steel, water quenched 855°C (1570°F), 540°C (1000°F) temper, 50 mm (2 in.) round
AISI 4130 Steel, water quenched 855°C (1570°F), 540°C (1000°F) temper, 13 mm (0.5 in.) round

M4130K / 7496

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.