MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC LNP™ STAT-LOY™ Compound M3000C Polypropylene, Unspecified (PP, Unspecified)
Categories: Polymer; Thermoplastic; Polypropylene (PP)

Material Notes: LNP STAT-LOY M3000C compound is based on unfilled Polypropylene (PP) resin containing proprietary fillers. Added features of this grade include: LNP Clean Compounding Technology, Permanently Anti-Static.

Features: LNP Clean Compound Technology,Antistatic

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.930 g/cc0.0336 lb/in³ASTM D792
 0.930 g/cc0.0336 lb/in³ISO 1183
Moisture Absorption 0.160 %0.160 %23°C/50% RH/24 hrs; ASTM D570
 0.160 %0.160 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.010 - 0.020 cm/cm0.010 - 0.020 in/in24hrs; ASTM D955
Linear Mold Shrinkage, Transverse 0.010 - 0.020 cm/cm0.010 - 0.020 in/in24hrs; ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 18.0 MPa2610 psi50 mm/min; ASTM D638
 24.0 MPa3480 psi50 mm/min; ISO 527
Elongation at Break 689 %689 %50 mm/min; ASTM D638
 690 %690 %50 mm/min; ISO 527
Tensile Modulus 0.760 GPa110 ksi50 mm/min; ASTM D638
 1.18 GPa171 ksi1 mm/min; ISO 527
Flexural Strength 24.0 MPa3480 psi1.3 mm/min, 50 mm span; ASTM D790
 38.0 MPa5510 psi2 mm/min; ISO 178
Flexural Modulus 0.860 GPa125 ksi1.3 mm/min, 50 mm span; ASTM D790
 1.96 GPa284 ksi2 mm/min; ISO 178
Izod Impact Notched 75.0 J55.3 ft-lbASTM D256
Izod Impact, Notched (ISO) 6.00 kJ/m²2.86 ft-lb/in²80*10*4; ISO 180/1A
Dart Drop, Total Energy 29.0 J21.4 ft-lbASTM D3763
Impact Test 25.0 J18.4 ft-lbMultiaxial Impact; ISO 6603
 
Electrical PropertiesMetricEnglishComments
Surface Resistance 1.00e+10 - 1.00e+12 ohm1.00e+10 - 1.00e+12 ohmASTM D257
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 128 µm/m-°C
@Temperature -30.0 - 30.0 °C
71.1 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM D696
CTE, linear, Transverse to Flow 131 µm/m-°C
@Temperature -30.0 - 30.0 °C
72.8 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 75.0 °C167 °FFlatw 80*10*4 sp=64mm; ISO 75/Bf
 74.0 °C
@Thickness 3.20 mm
165 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 49.0 °C120 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 49.0 °C
@Thickness 3.20 mm
120 °F
@Thickness 0.126 in
unannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Zone 2 195 - 205 °C383 - 401 °F
Zone 3 200 - 210 °C392 - 410 °F
Melt Temperature 190 - 200 °C374 - 392 °FInjection Molding
Mold Temperature 30.0 - 50.0 °C86.0 - 122 °F
Drying Temperature 70.0 - 80.0 °C158 - 176 °FInjection Molding
Dry Time 4.00 hour4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa29.0 - 43.5 psi
Screw Speed 30 - 60 rpm30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH81418 / 289365

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.