MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Avient Bergamid™ A70 G30 U Polyamide 66 (Nylon 66)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66)

Material Notes:

Information provided by PolyOne

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.60 g/cc±0.03 g/cm³; ISO 1183
Filler Content 30 %Glass Fiber Reinforcement
Water Absorption 0.030 %
@Thickness 3.18 mm
@ 24 hrs; ASTM D570
Linear Mold Shrinkage, Flow 0.0010 - 0.0020 cm/cmASTM D955
Ash 30 %ISO 3451
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 170 MPa
@Temperature 23.0 °C
ISO 527-2/5
Elongation at Break 2.0 %
@Temperature 23.0 °C
ISO 527-2/5
Tensile Modulus 11600 MPa
@Temperature 23.0 °C
ISO 527-2/1
Charpy Impact Unnotched 55.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 8.00 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+12 ohm-cmIEC 60093
Surface Resistance 1.00e+10 ohmIEC 60093
Comparative Tracking Index 300 VSolution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
Melting Point 261 °CISO 3146
Maximum Service Temperature, Air 130 °CContinuous (GTP 50% Tensile); IEC 60216
 220 °CShort Time; IEC 60216
Deflection Temperature at 0.46 MPa (66 psi) 250 °CUnannealed; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 250 °CUnannealed; ISO 75-2/A
Flammability, UL94 V-0
@Thickness 0.800 mm
UL 94
Glow Wire Flammability Index 960 °C
@Thickness 1.60 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Melt Temperature 265 - 290 °C
Mold Temperature 60.0 - 90.0 °C
 
Descriptive Properties
FeaturesFlame Retardant
 Halogenated
FormsPellets
Generic MaterialNylon 66
Generic NamePolyamide 66 (Nylon 66)
Processing MethodInjection Molding
Regional AvailabilityEurope
RoHS ComplianceRoHS Compliant

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Nilit Nilamid A3 H6 G5 25% Glass Reinforced PA66
LATI Kelon® B FR H2 CEG/500-V0CT3 PA 6, Glass/Mineral Reinforced, Flame Retardant, Heat Stabilized
LATI Later 4 G/30-V0 PBT, 30% Glass Fiber Reinforced, Flame Retardant
LATI Laticonther 62 CEG/500-V0HF1 PA 6, Glass/Mineral Reinforced, Flame Retardant
Overview of materials for Nylon 6, Impact Grade

PH0POL1226 / 145795

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.