MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Dow AMPLIFY™ EA 101 Ethylene-ethyl Acrylate (EEA)  (discontinued **)
Categories: Polymer; Thermoplastic

Material Notes: AMPLIFY™ EA 101 Functional Polymer is produced via a high pressure reactor. It exhibits high flexibility and imparts low temperature toughness to a wide range of engineering resins. This polymer demonstrates excellent blend compatibility with other polyolefins. It can be utilized as a tie layer between polyolefins and a variety of polar substrates, such as metal, polyvinylidiene chloride (PVDC), polyolefins, cellulose, polyester, polycarbonate, glass, foil, PVC, PET, and Polystyrene.

Information provided by Dow

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.931 g/ccASTM D792
Filler Content 18.5 %Comonomer; ASTM D4094
Melt Flow 6.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 86ASTM D2240
Hardness, Shore D 31ASTM D2240
Tensile Strength, Ultimate 1950 psiASTM D638
Tensile Strength, Yield 430 psiASTM D638
Elongation at Break 750 %ASTM D638
Elongation at Yield 10 %ASTM D638
Flexural Modulus 8000 psi
@Strain 2 %
Secant; ASTM D790
Tensile Impact Strength 320 ft-lb/in²ASTM D1822, Type S
 
Thermal PropertiesOriginal ValueComments
Melting Point 98.0 °CDow Method
Crystallization Temperature 83.0 °CDow Method
Deflection Temperature at 0.46 MPa (66 psi) 88.0 °FASTM D648
Vicat Softening Point 135 °FASTM D1525
Brittleness Temperature <= -76.0 °CASTM D746

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Dow AMPLIFY™ EA 100 Ethylene-ethyl Acrylate (EEA)
Dow AMPLIFY™ EA 102 Ethylene-ethyl Acrylate (EEA)
Dow AMPLIFY™ EA 103 Ethylene-ethyl Acrylate (EEA)
Dow Elvaloy® AC 2618 Ethylene Methyl Acrylate
Dow Elvaloy® 4170 Reactive Ethylene Terpolymer (RET)

PDOW1181 / 30399

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.