MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Chi Mei Polyrex® PH-88S Polystyrene - Extrusion
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Extrusion Grade

Material Notes: Extrusion

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/ccISO 1183
Melt Flow 3.0 g/10 min
@Load 10.0 kg,
Temperature 220 °C
Melt Volume Rate (ml/10 min); ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 76.0 MPaH358/30; ISO 2039-1
Tensile Strength at Break 24.0 MPa50 mm/min; ISO 527
Tensile Strength, Yield 25.0 MPa50 mm/min; ISO 527
Elongation at Break 66 %50 mm/min; ISO 527
Flexural Strength 34.0 MPa2 mm/min; ISO 178
Flexural Modulus 1.40 GPa2 mm/min; ISO 178
Izod Impact, Notched (ISO) 13.0 kJ/m²ISO 180/1A
Izod Impact, Unnotched (ISO) NBISO 180/1C
Charpy Impact Unnotched NBISO 179
Charpy Impact, Notched 1.40 J/cm²ISO 179
Impact 14Impact Flexural Test Notched (KJ/m²)
 100Impact Flexural Test Unnotched (KJ/m²)
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 77.0 °Cunannealed; ISO 75
 94.0 °Cannealed; ISO 75
Vicat Softening Point 89.0 °C
@Load 5.00 kg
50°C/hr; ISO 306
 93.0 °C
@Load 5.00 kg
120°C/hr; ISO 306
 100 °C
@Load 1.00 kg
50°C/hr; ISO 306
 104 °C
@Load 1.00 kg
120°C/hr; ISO 306
Flammability, UL94 HB
@Thickness 1.59 mm
UL 94

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chi Mei Polyrex® PH-888H Polystyrene - High Impact
Chi Mei Polyrex® PG-22 Polystyrene
Chi Mei Polyrex® PG-33 Polystyrene
Chi Mei Polyrex® PG-383 Polystyrene
Chi Mei Polyrex® PG-80 Polystyrene

PCHI942 / 109430

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.