MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Domo TECHNYL® eXten D 458P PA6.10, DRY
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 610 (PA610)

Material Notes: Description: Product in development - provisional datasheet. High viscosity unfilled plasticized PA6.10 for extrusion applications providing low end part warpage.

Available in: Asia Pacific, Europe, Latin America and North America

Product Applications: Polyamide 6,10 for extrusion, where high flexibility and toughness are requested, especially low temperature toughness. TECHNYL® eXten D 458P is specially developed for automotive and other applications where a long term high temperature usage is requested. This material is available in black and natural.

DOMO Chemicals has acquired Solvay’s Performance Polyamides Business in Europe.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.04 g/cc0.0376 lb/in³ISO 1183/A
Water Absorption 0.46 %
@Time 86400 sec
0.46 %
@Time 24.0 hour
ISO 62
Water Absorption at Saturation 1.75 %1.75 %ISO 62
Viscosity  0.20 cP
@Shear Rate 1500 1/s,
Temperature 230 °C
0.20 cP
@Shear Rate 1500 1/s,
Temperature 446 °F
 1.0 cP
@Shear Rate 300 1/s,
Temperature 230 °C
1.0 cP
@Shear Rate 300 1/s,
Temperature 446 °F
 1.5 cP
@Shear Rate 100 1/s,
Temperature 230 °C
1.5 cP
@Shear Rate 100 1/s,
Temperature 446 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 6363ISO 868
Tensile Strength at Break 40.0 MPa5800 psiISO 527 Type 1A
Tensile Strength, Yield 33.0 MPa4790 psiISO 527 Type 1A
Tensile Stress at Strain  10.0 MPa
@Strain 3 %,
Temperature 80.0 °C
1450 psi
@Strain 3 %,
Temperature 176 °F
 10.0 MPa
@Strain 10 %,
Temperature 135 °C
1450 psi
@Strain 10 %,
Temperature 275 °F
 10.0 MPa
@Strain 1 %,
Temperature 23.0 °C
1450 psi
@Strain 1 %,
Temperature 73.4 °F
 10.0 MPa
@Strain 15 %,
Temperature 150 °C
1450 psi
@Strain 15 %,
Temperature 302 °F
 12.0 MPa
@Strain 20 %,
Temperature 150 °C
1740 psi
@Strain 20 %,
Temperature 302 °F
 12.0 MPa
@Strain 20 %,
Temperature 135 °C
1740 psi
@Strain 20 %,
Temperature 275 °F
 17.0 MPa
@Strain 120 %,
Temperature 135 °C
2470 psi
@Strain 120 %,
Temperature 275 °F
 18.0 MPa
@Strain 200 %,
Temperature 150 °C
2610 psi
@Strain 200 %,
Temperature 302 °F
 20.0 MPa
@Strain 3 %,
Temperature 23.0 °C
2900 psi
@Strain 3 %,
Temperature 73.4 °F
 20.0 MPa
@Strain 20 %,
Temperature 80.0 °C
2900 psi
@Strain 20 %,
Temperature 176 °F
 22.0 MPa
@Strain 100 %,
Temperature 80.0 °C
3190 psi
@Strain 100 %,
Temperature 176 °F
 30.0 MPa
@Strain 10 %,
Temperature 23.0 °C
4350 psi
@Strain 10 %,
Temperature 73.4 °F
 35.0 MPa
@Strain 20 %,
Temperature 23.0 °C
5080 psi
@Strain 20 %,
Temperature 73.4 °F
 40.0 MPa
@Strain 152 %,
Temperature 23.0 °C
5800 psi
@Strain 152 %,
Temperature 73.4 °F
Elongation at Break >= 200 %>= 200 %ISO 527 Type 1A
Tensile Modulus 0.850 GPa123 ksiISO 527 Type 1A
Flexural Modulus 0.690 GPa100 ksiISO 178
Charpy Impact Unnotched NBNBISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched  1.30 J/cm²
@Temperature -30.0 °C
6.19 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 10.0 J/cm²
@Temperature 23.0 °C
47.6 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 215 °C419 °FISO 11357
Deflection Temperature at 1.8 MPa (264 psi) 51.0 °C124 °FISO 75/Af
 
Processing PropertiesMetricEnglishComments
Feed Temperature 205 - 225 °C401 - 437 °F
Front Barrel Temperature 220 - 240 °C428 - 464 °F
Die Temperature 215 - 235 °C419 - 455 °F
Drying Temperature 80.0 °C
@Time 28800 sec
176 °F
@Time 8.00 hour
Moisture Content <= 0.10 %<= 0.10 %
 
Descriptive Properties
Compression Zone225-235°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Domo TECHNYL® eXten D 458P PA6.10, Conditioned
Shakespeare Isocor™ HW115SI Nylon 610
Shakespeare Isocor™ HW29TL Nylon 610
Shakespeare Isocor™ HW69SI Nylon 610
Shakespeare Isocor™ SVP6100 Nylon 610

PRHOD558 / 137789

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.