MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Celanese Crastin® SK643FR NC010 Polybutylene Terephthalate (PBT)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled

Material Notes: 20% Glass Reinforced Flame Retardant Polybutylene Terephthalate

Crastin SK643FR is a flame retardant 20% glass reinforced polybutylene terephthalate molding resin. It is recognized as UL94V-0 at 0.8mm.

Former DuPont product acquired by Celanese in 2022.

Key Words: PBT-GF20FR(17)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.63 g/cc0.0589 lb/in³ISO 1183
Water Absorption 0.30 %
@Thickness 2.00 mm
0.30 %
@Thickness 0.0787 in
Sim. to ISO 62
Moisture Absorption 0.150 %
@Thickness 2.00 mm
0.150 %
@Thickness 0.0787 in
Sim. to ISO 62
Viscosity Number 100 cm³/g1.00 dl/gISO 307, 1157, 1628
Linear Mold Shrinkage, Flow 0.0050 cm/cm0.0050 in/inISO 294-4, 2577
 0.0060 cm/cm0.0060 in/inannealed; ISO 294-4
 0.0010 cm/cm
@Treatment Temp. 80.0 °C,
Time 173000 sec
0.0010 in/in
@Treatment Temp. 176 °F,
Time 48.0 hour
Postmolding shrinkage; ISO 294-4
Linear Mold Shrinkage, Transverse 0.012 cm/cm0.012 in/inISO 294-4, 2577
 0.0145 cm/cm0.0145 in/inannealed; ISO 294-4
 0.0030 cm/cm
@Treatment Temp. 80.0 °C,
Time 173000 sec
0.0030 in/in
@Treatment Temp. 176 °F,
Time 48.0 hour
Postmolding shrinkage; ISO 294-4
Melt Flow  6.0 g/10 min
@Load 2.16 kg,
Temperature 250 °C
6.0 g/10 min
@Load 4.76 lb,
Temperature 482 °F
cm³/10min Volumetric; ISO 1133
 9.0 g/10 min
@Load 2.16 kg,
Temperature 250 °C
9.0 g/10 min
@Load 4.76 lb,
Temperature 482 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 113 MPa16400 psiISO 527-1/-2
Elongation at Break 3.0 %3.0 %ISO 527-1/-2
Tensile Modulus 8.50 GPa1230 ksiISO 527-1/-2
Flexural Strength 170 MPa24700 psiISO 178
Poissons Ratio 0.340.34
Izod Impact, Notched (ISO)  7.00 kJ/m²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
ISO 180/1A
 8.00 kJ/m²
@Temperature 23.0 °C
3.81 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1A
Izod Impact, Unnotched (ISO)  35.0 kJ/m²
@Temperature -30.0 °C
16.7 ft-lb/in²
@Temperature -22.0 °F
ISO 180/1U
 36.0 kJ/m²
@Temperature 23.0 °C
17.1 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1U
Charpy Impact Unnotched  5.30 J/cm²
@Temperature -30.0 °C
25.2 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
 5.50 J/cm²
@Temperature 23.0 °C
26.2 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  0.780 J/cm²
@Temperature -30.0 °C
3.71 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 0.850 J/cm²
@Temperature 23.0 °C
4.04 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
Tensile Creep Modulus, 1 hour 7200 MPa1.04e+6 psi1h; ISO 899-1
Tensile Creep Modulus, 1000 hours 5500 MPa798000 psi1000h; ISO 899-1
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmIEC 62631-3-1
Surface Resistance 1.00e+15 ohm1.00e+15 ohmIEC 62631-3-2
Dielectric Constant  3.7
@Frequency 1e+6 Hz
3.7
@Frequency 1e+6 Hz
IEC 62631-2-1
 3.8
@Frequency 100 Hz
3.8
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 28.0 kV/mm711 kV/inIEC 60243-1
Dissipation Factor  0.0030
@Frequency 100 Hz
0.0030
@Frequency 100 Hz
IEC 62631-2-1
 0.016
@Frequency 1e+6 Hz
0.016
@Frequency 1e+6 Hz
IEC 62631-2-1
Comparative Tracking Index 250 V250 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 40.0 µm/m-°C22.2 µin/in-°FISO 11359-1/-2
CTE, linear, Transverse to Flow 100 µm/m-°C55.6 µin/in-°FISO 11359-1/-2
Melting Point 224 °C435 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 220 °C428 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 205 °C401 °FISO 75-1/-2
Glass Transition Temp, Tg 55.0 °C131 °F10°C/min; ISO 11357-1/-2
Flammability, UL94  V-0
@Thickness 0.750 mm
V-0
@Thickness 0.0295 in
IEC 60695-11-10
 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
IEC 60695-11-10
Oxygen Index 31 %31 %ISO 4589-1/-2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 250 °C482 °FOptimum, Injection
 240 - 260 °C464 - 500 °FRange, Injection
Mold Temperature 80.0 °C176 °FOptimum, Injection
 30.0 - 130 °C86.0 - 266 °FInjection
Ejection Temperature 170 °C338 °FInjection
Drying Temperature 120 °C248 °FInjection
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.040 %<= 0.040 %Injection
Hold Pressure >= 60.0 MPa>= 8700 psiInjection
 
Descriptive Properties
AdditivesFlame retardant
Back pressureAs low as possible
Drying RecommendedyesInjection
FMVSS ClassDNIISO 3795 (FMVSS 302)
Part Marking Code>PBT-GF20FR(17)<ISO 11469
PolymerPBT-GF20 FR(17)
Processing Hold Pressure Time (s/mm)3Injection
Resin IdentificationPBT-GF20FR(17)ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Crastin® SK643FR BK851 PBT-GF20FR(17)
Celanese Crastin® FGS600F40 NC010 PBT
BASF Ultradur® B 4300 G4 20% Glass Filled PBT
Celanese Crastin® S600F20 NC010 PBT
Celanese Crastin® S610SF NC010 PBT

PDSY5084 / 160911

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.